Based off your measurements I would estimate you need 700-750g of resin.
Fibre:resin ratio should be ~60:40, so you need about 450g of resin (I like to round up) for your 650g of reinforcement.
Mesh will take about 700g per square metre. Peel ply is pretty negligible unless you are doing bigger infusions, its about 80g/sqm. By rounding each calculation up, I find you tend to compensate enough to not worry about calculating for peel ply, and hoses, and then depending on infusion size I might factor in a little bit of wastage in the bottom of the pot as well.
|