This was a practice run at resin infusion. I had never tried it and wanted to see how it went. Overall I learned a lot (mostly what not to do) and this was the result. Panel is 3 plys of 3k 2x2 twill, on a glass table top that was waxed with 5 coats of Partall #2.

I'm wondering if anyone can help identify the cause of the couple of dull spots on the panel. Perhaps the resin didn't penetrate all of the way through? Issue with using just wax? Pinhole leak in the bag?



I tried to grab a slightly more up close shot:


Thanks for the help as always!



Replies
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Yeh looks like a slight release issue, which isn't uncommon with wax on glass. Wax doesn't bond well to glass, so it often isn't a suitable release agent on its own (when used on glass). Ideally you want a chemical release agent.
AlpineCoupe
A
Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)Supreme Being (429 reputation)
Group: Forum Members
Posts: 45, Visits: 2.1K
Hanaldo - 1/22/2021 2:03:04 PM
Yeh looks like a slight release issue, which isn't uncommon with wax on glass. Wax doesn't bond well to glass, so it often isn't a suitable release agent on its own (when used on glass). Ideally you want a chemical release agent.

Thanks! I have some 700nc that I'll try instead of the wax. 