Trying to figure out how to keep the bag to stay tight all the way through the infusion process. there’s absolutely no leaks before we start infusing the resin. But as soon as we open up the resin inlet line the inlet side/area of the bag loosens up and it really never get a tight until the resin starts to gel. Anyone have this issue or does anyone know how to fix this issue. I’m finding small pitting on the surface and only on the inlet side so i’m guessing g it’s happening from the bag being loose on that side.
Replies
FrankZane
F
Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)
Group: Forum Members
Posts: 1, Visits: 6
Loss of bag tightness is caused by the pressure gradient between the vacuum port and the resin port.
the resin port needs to be restricted to prevent it's pressure dropping to ambient.
Link below shows this phenomenon.
https://www.youtube.com/watch?v=4In9_Eyz6gs
MarkMK
MarkMK
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 338, Visits: 2K
I'd be a touch wary of taking-in everything you might see on You Tube and potentially introducing methods that are unnecessary and counter-productive

I'm not doubting the findings, but I don't think that it offers anything in the way of delivering a better result and it is not necessary to restrict the inlet flow at all. It would be misleading to imply it was somehow necessary when infusing parts

Looseness in the bag around the inlet when resin begins to flow is not an issue to worry about, as mentioned earlier and assuming that the bag is perfectly sealed, everything will tighten once the part is closed-off and pressure equalises. 

I've infused hundreds of parts to date, many of them quite small and relatively quick to wet-out and have always had a consistently perfect cosmetic finish. The use of resin breaks sized in proportion to the part size/infusion speed and allowing a small amount of resin flow after closing-off the vacuum port has been more than enough to ensure those consistent results. 

I've not yet encountered a single scenario where choking the resin flow would have been desirable. 

On smaller parts, in particular, choking the resin flow tends to lead to the gas in the resin becoming greatly expanded as the vacuum pressure at the front has a bigger impact. Whilst this might reduce when both ports are closed-off as pressure equalises over the whole part, it feels an undesirable method of trying to achieve a void free finish, especially where resin is likely to reach the exit fairly quickly.

The appearance of the gas is likely to be far more prominent and not just at the front. At the extreme, it's only been the sudden appearance of lots of large bubbles across an part being infused that's alerted me to the fact that the bottom of the inlet tube has vacuum sealed itself to the base of the resin pot. 

As an aide and it's been debated a few times before, I don't bother with degassing any more either, prior to infusion, as I've found that it doesn't deliver a completely gas-free resin or impact on the part's cured cosmetic finish. Some swear by it, but I've yet to find any cosmetic difference in results, even on more complex-shaped parts.

The OP's issue was voids and/or dry areas around the inlet, which seems to indicate a slight starvation of resin in this area, so it appears that his previous process might have been restricting the flow of resin towards the end of the infusion. I don't think that introducing a restriction of resin flow would help matters at all and would be more likely to introduce unwanted cosmetic issues 


Edited 6 Years Ago by MarkMK
mscomposites
m
Supreme Being (215 reputation)Supreme Being (215 reputation)Supreme Being (215 reputation)Supreme Being (215 reputation)Supreme Being (215 reputation)Supreme Being (215 reputation)Supreme Being (215 reputation)Supreme Being (215 reputation)Supreme Being (215 reputation)
Group: Forum Members
Posts: 23, Visits: 108
thanks for the advice again MarkMK We have been getting almost near perfect parts once we lowered our resin pot lower than the mold and restricting the resin flowing in just a little bit. Not to the point where the part looks like it’s starving but just enough to keep the bag tight through out the whole process. We also started degassing the resin upfront seems like that also eliminated a lot of the small surface pitting that we were getting. Those were the only two things we changed and we are getting better results now. Not sure if if it’s one or the other that gave us the results or both of them togeather. I usually like to only change one thing at a time but we just didn’t have anymore testing time, we had to start producing parts. We also noticed that the parts would come out pit free but as soon as we cleaned them up to spray our flat clear coat on them (per customers choice) the acetone we were cleaning the parts with was actually removing resin off the surface and breaking into the fabric and causing surface pores. Needless to say no more cleaning of the parts with knarly solvants.
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
mscomposites - 6 Years Ago
Hanaldo - 6 Years Ago
mscomposites - 6 Years Ago
mscomposites - 6 Years Ago
SleepingAwake - 6 Years Ago
mscomposites - 6 Years Ago
MarkMK - 6 Years Ago
mscomposites - 6 Years Ago
SleepingAwake - 6 Years Ago
MarkMK - 6 Years Ago
FrankZane - 6 Years Ago
MarkMK - 6 Years Ago
mscomposites - 6 Years Ago
Hanaldo - 6 Years Ago
mscomposites - 6 Years Ago
mscomposites - 6 Years Ago
Hanaldo - 6 Years Ago
mscomposites - 6 Years Ago
Hanaldo - 6 Years Ago
mscomposites - 6 Years Ago
SleepingAwake - 6 Years Ago
mscomposites - 6 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search