Paint and Gel Coat?


Author
Message
ian.g
i
Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)
Group: Forum Members
Posts: 22, Visits: 96
I am using a MDF mould buck which I need to 'smooth' with primer and top coat of paint - I propose to use a nitro-acrylic paint - will that work with a gel coat and polyester resin which will be used to make the mould?

Thanks
JasonFL
JasonFL
Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)
Group: Forum Members
Posts: 51, Visits: 707
ian.g - 4/5/2019 10:00:12 PM
I am using a MDF mould buck which I need to 'smooth' with primer and top coat of paint - I propose to use a nitro-acrylic paint - will that work with a gel coat and polyester resin which will be used to make the mould?Thanks


Why not use a Polyester primer like Duratec, sand it to 1000 grit finish, then polish with Aquabuff to a shine?

Jason
ian.g
i
Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)
Group: Forum Members
Posts: 22, Visits: 96
Thanks for the suggestion - Is there a document anyone knows of which ‘lists’ compatibility of finishes with polyester and epoxy?

Are polyester abs epoxy compatible? So can I bond polyester glassfibre parts into a CF part or do I use epoxy and glassfibre for that or should I only add epoxy CF to a CF part?

Bit confused about the compatibility rules!!
JasonFL
JasonFL
Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)
Group: Forum Members
Posts: 51, Visits: 707
Polyester and Epoxy are compatible.

Polyester and Urethanes are for a very short time period. If the poly is under the urethane it will off gas and eventually create bubbles in the urethane and ruin your plug. I ruined many, many plugs this way before some one mentioned the compatibility issues.

When building plugs Polyester primer is all you need. It can be polished to a mirror. Really is no reason to use anything else.

For bonding always use epoxy and under 100 grit sand paper for prep. You’re relying on a mechanical bond if youre bonding post cure. Bigger scratches for the epoxy to bite into, the better.

Jason
ian.g
i
Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)
Group: Forum Members
Posts: 22, Visits: 96
JasonFL - 4/13/2019 2:43:49 PM
Polyester and Epoxy are compatible. Polyester and Urethanes are for a very short time period. If the poly is under the urethane it will off gas and eventually create bubbles in the urethane and ruin your plug. I ruined many, many plugs this way before some one mentioned the compatibility issues.When building plugs Polyester primer is all you need. It can be polished to a mirror. Really is no reason to use anything else.For bonding always use epoxy and under 100 grit sand paper for prep. You’re relying on a mechanical bond if youre bonding post cure. Bigger scratches for the epoxy to bite into, the better.

So I'm not using Urethanes but Acrylic - didn't manage to find any polyester primer in time - but acrylic paint seems to be compatible when over-slapped with gel coat/ polyester resin/glass fibre?

The mould will therefore be polyester and I will fill it with Epoxy Carbon Fibre - all as per the bonnet EasyComposite tutorial... which is extremely clear!
I think I will bond the steel in with the lay-up of the carbon fibre so there is a chemical bond over and around the steel for maximum rigidity - good idea or not?
Final piece of the puzzle - when I connect the top and bottom parts I will have a hollow piece which I want to fill with some kind of expanding foam - anybody done this?

Thanks for all your help so far - great forum!






JasonFL
JasonFL
Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)
Group: Forum Members
Posts: 51, Visits: 707
I’m not sure what youre using the steel for. Is it to add rigidity to a mould or a finished part?

If for a mould, youll need to insulate the steel with E glass to protect it from the Carbon, OR, completely seal the steel off from any oxygen exposure to prevent galvanic corrosion.

Also, sand the steel with 40 or 50 grit paper thoroughly. Clean it in uni directional wipes with acetone multiple times. Using a swirling motion just spreads residual dirt and grease around the metal. Add the metal to the layup shortly after the acetone evaporates.

The foam idea sounds good. Is it needed though? Also are you using it to add structure or floatation? Use 2 pound foam for floatation, and 4 pound or higher if youre looking to add some rigidity.

Jason
ian.g
i
Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)
Group: Forum Members
Posts: 22, Visits: 96
JasonFL - 4/13/2019 6:47:24 PM
I’m not sure what youre using the steel for. Is it to add rigidity to a mould or a finished part?If for a mould, youll need to insulate the steel with E glass to protect it from the Carbon, OR, completely seal the steel off from any oxygen exposure to prevent galvanic corrosion. Also, sand the steel with 40 or 50 grit paper thoroughly. Clean it in uni directional wipes with acetone multiple times. Using a swirling motion just spreads residual dirt and grease around the metal. Add the metal to the layup shortly after the acetone evaporates.The foam idea sounds good. Is it needed though? Also are you using it to add structure or floatation? Use 2 pound foam for floatation, and 4 pound or higher if youre looking to add some rigidity.

The steel is to add a bit of 'heft' to the finished part, for fixings and to provide extra rigidity along its axis!
I was planning to encase the steel in the carbon fibre to cut off the oxygen...would the steel corrode in contact with the carbon - even if the carbon fibre is impregnated with resin? I will clean it as suggested - presumably to aid bonding?
The foam is to stop the part from sounding hollow and to add some rigidity - what sort of expanding foam should I use - like the stuff for sealing holes on buildings?
Many thanks!
Ian

JasonFL
JasonFL
Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)
Group: Forum Members
Posts: 51, Visits: 707
if there is an epoxy surface coat you have nothing to worry about. If it’s epoxy and carbon without a finish then it will corrode over time.

I’d use two part expanding foam with a 4 pound density. I’d avoid the stuff in a spray can.

Jason
oekmont
oekmont
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 550, Visits: 27K
Sorry to interrupt, but acrylic paint isn't a good option to finish the plug. Even with epoxy there are problems, but the styrene in the polyester will attack the paint heavily, and your mould will be wasted.
If you haven't got the equipment to spay a 2k primer, you could use a polyester brush/roll primer, like the one from ec.
"Polyester and epoxy are compatible" is a dangerous sentence. Epoxy bonds to polyester quite well, but polyester doesn't bond to epoxy.
If you want the steel for extra weight, a few layers of thick glass cloth could be an easier and saver option. If you want to use the steel for fixing, it will obviously be exposed. You should always protect steel from the carbon. Never laminate c.f. directly on steel. Either use a thin glass cloth as first layer, or use special ep or urethane primer first.


ian.g
i
Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)Supreme Being (151 reputation)
Group: Forum Members
Posts: 22, Visits: 96
Thanks for all the useful advice!

I have a problem now because the buck is now painted with acrylic-nitro - I had read that Polyester on acrylic was ok but not the other way around. Can I use an epoxy on the acrylic paint? Hopefully I don’t need to strip all the paint off - that would be a job...

I will cover the steel with a pure epoxy coat before bonding it into the piece in a second epoxy carbon fibre hand lay operation.

Then I will join the front and back with epoxy adhesive.

Then I will make some holes and inject some 4 pound resin.

Thanks

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search