Glasscast 50. Pouring onto an already cured river table


Author
Message
Dsully
D
Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)
Group: Forum Members
Posts: 5, Visits: 19
Hi guys. I've just poured my first river table with some nice oak. I Maybe didn't leave enough time between pours as the temperature is 13/14 degrees. It was probably too sticky still. Anyways its shrunk and I need more resin to Complete the table. It's my first time ever working with resin. If anyone has tips about pouring onto an already cured river would be greatly appreciated. Be it sanding etc. Thanks, Daniel 
Replies
Rich (Staff)
Rich (Staff)
Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)
Group: Administrators
Posts: 167, Visits: 4.6K
Hi Dsully, As I'm sure you know, the best option is actually to pour subsequent layers when the previous has reached the 'B' or 'Tack' stage of cure whereby the resin feels tacky to the touch but, when wearing gloves, no residue is lifted off on your fingertips, however, if this stage is missed then you need to wait for full cure and once fully hardened, abrade the surface with a 120-240grit abrasive paper, remove any dust and then pour the subsequent layer. The new layer will infill all of the surface scratches left in the keying process to again give a seamless bond.

Dsully
D
Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)
Group: Forum Members
Posts: 5, Visits: 19
Rich (Staff) - 2/4/2019 2:47:04 PM
Hi Dsully, As I'm sure you know, the best option is actually to pour subsequent layers when the previous has reached the 'B' or 'Tack' stage of cure whereby the resin feels tacky to the touch but, when wearing gloves, no residue is lifted off on your fingertips, however, if this stage is missed then you need to wait for full cure and once fully hardened, abrade the surface with a 120-240grit abrasive paper, remove any dust and then pour the subsequent layer. The new layer will infill all of the surface scratches left in the keying process to again give a seamless bond.

Thanks alot for the advice Rich, much appreciated πŸ‘

Dsully
D
Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)Forum Guru (62 reputation)
Group: Forum Members
Posts: 5, Visits: 19
Rich (Staff) - 2/4/2019 2:47:04 PM
Hi Dsully, As I'm sure you know, the best option is actually to pour subsequent layers when the previous has reached the 'B' or 'Tack' stage of cure whereby the resin feels tacky to the touch but, when wearing gloves, no residue is lifted off on your fingertips, however, if this stage is missed then you need to wait for full cure and once fully hardened, abrade the surface with a 120-240grit abrasive paper, remove any dust and then pour the subsequent layer. The new layer will infill all of the surface scratches left in the keying process to again give a seamless bond.

Hi mate, what would you recommend to Clean it with after removing the dust

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Dsully - 6 Years Ago
Bhamoggy - 6 Years Ago
Dsully - 6 Years Ago
Rich (Staff) - 6 Years Ago
Dsully - 6 Years Ago
Dsully - 6 Years Ago
Warren (Staff) - 6 Years Ago
             Cheers mate
Dsully - 6 Years Ago
Graham Burdett - 4 Years Ago
Warren (Staff) - 4 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search