Can't prevent pitholes


Author
Message
BMac
B
Supreme Being (144 reputation)Supreme Being (144 reputation)Supreme Being (144 reputation)Supreme Being (144 reputation)Supreme Being (144 reputation)Supreme Being (144 reputation)Supreme Being (144 reputation)Supreme Being (144 reputation)Supreme Being (144 reputation)
Group: Forum Members
Posts: 16, Visits: 63
I have tried 3 times to put a final coat on my carbon skinned parts but I still keep getting air bubbles and pitholes.
I have sanded, cleaned, 3-1 mix and all new brushes etc. I'm using the xcr resin.
Below are the photos. Can anyone help.

Reply
Geteda
Geteda
Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)
Group: Forum Members
Posts: 15, Visits: 58
you must mix slowly about 3 minutes and then degas the resin to full vacuum about 4 minutes, the mixture / viscosity
in this resin xcr is 856cps, it is easy to trap air. You can try to put a final coat with lower viscocity resin.. the bubbles goes fast.