	Group: Administrators 	        
    Posts: 134, 
    Visits: 614 
    
 
          
		     | 
				                       
                 
                
                    
			            Hi, 
  The Permabond 515 will bond vinylester parts very well, obviously you would need to prepare the area like any other (sand and degrease) 
  As a rule of thumb these guidlines can be followed for resin bonding; 
  Epoxy will bond well to cured polyester/vinylester Vinylester/polyester will bond reasonably well to itself  Vinylester/polyester will not bond well to cured epoxy  Epoxy will bond well to itself 
  The ET515 is an epoxy based adhesive so it should adhere well to any resin system.                
			            
  				
			            Paul Statham Easy Composites / Carbon Mods - Technical                     
                     
                                            
                         
                    
                  
             |