Initially try heat to see if it forces the resin to cure. Otherwise Honaldo is right in that you would need to remove the uncured resin and re-pour fresh. Depending exactly how bad it is, it may well be virtually impossible to remove it all without damaging the embedded pennies.
Use a sander to quickly take down the resin but stop just short of the pennys. At that point reassess. If its all hard resin then you are ok. If it is still jelly/gloopy liquid in places, if you have access, mop it up, clean with acetone until everything is dry and you should be ok.
Its a lot of work but in most cases it is doable to recover to a point you can pour again.