Hi guys, I am still learning and I have been using a small mould as a test.  I have just pulled my small money tray made of 2x2 twill carbon out of the mould and there are tiny pinholes on one side of the surface, I am sure that the bag kept full vac all the way through the infusion so my question is what are the main reasons for a pinhole finish. 

I have been working in the garage which is cold but have my mould on an electric blanket to keep it warm.  the only thing different with this infusion is that I didn't use any spray tack on the surface. 

I am quite happy to have these little problems as I want to learn as much as I can but I need to have an understanding of why things happen and how to improve.

Thanks in advance

Nothing good to say......then say nothing
Reply
LeeBrett
LeeBrett
Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)
Group: Forum Members
Posts: 11, Visits: 167
Thanks guys, its a bit hard to see from the picture as I found it very hard get a good picture of the tiny pinholes on the surface.  I think that the infusion probably went a bit too fast as when I opened the inlet line the pipe was sucked closed and when I squeezed the kink the resin rapidly shot in but seemed like it had good coverage.  I think I will try again this time going really slowly. 

Also I  will be looking into making my own de gassing pot.

Nothing good to say......then say nothing
Attachments
pinholes.jpg (631 views, 100.00 KB)
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search