5 kg of chop matt = 20kg of resin the question is


Author
Message
Daz
Daz
Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)
Group: Forum Members
Posts: 93, Visits: 651
Do i need 1.6 kg of mekp to be the right mix ?

Im using the unimold system ,,

Thats what i have worked out i need

The mold is 67 inches by 50 inches which i have worked out to 2.16 sq meters

I only have 10kg of resin im thinking i need 20 kg

Is this correct or are my sums wrong ????
Edited 13 Years Ago by Daz
Reply
Paul (Staff)
Paul (Staff)
Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)
Group: Administrators
Posts: 134, Visits: 614
Hi Daz,

@2% you need 20g per 1kg of tooling resin so for 10kg that would be 200g, therefore 20kg needs 400g which you can do by volume and still be accurate enough so that's 400ml.

2.16sqm will use about 3.9kg of chopped strand mat (2.16[total surface area] x450[weight per sqm of the matting] x4[number of layers] = 3.888 ~^ 3.9) a good rule of thumb with the tooling resin is to double the weight of resin to the mat so this comes out at 7.8kg, you will need some left to have in reserve if it consumes more than expected so a 10kg pack would be right for that job.

Mix it up in 2kg batches as your working as this will mean that you won't have a big catalysed batch in the bucket, which could exotherm and cure quicker than you are working! 

Paul Statham
Easy Composites / Carbon Mods - Technical
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search