Has anyone had this happen? This is the first time I have used a pigment additive in my epoxy and also the first time using a liquid mold release called Frekote 700nc. I was attempting to apply my first coat of epoxy to my plug as I have done on my first plug with good results. As soon as I started to brush it on, it started to separate. I was able to wipe it off very easly before it cured. However, I am wondering if it could have been the pigment additive.

This is only the second mold that I have done. The first one worked fine other than my plug construction, and plug surface quality was poor. So, this time, I did a lot research on construction techniques and proper plug surface requirements. After reading about different mold release types, I choose to use a liquid type. From what I have read, you can achieve a better molded part surface finish.

Any input would be great.

Thanks,

Lee Adams



Lee Adams

www.melleen.com

info@melleen.com
Replies
Brian_s
Brian_s
Supreme Being (793 reputation)Supreme Being (793 reputation)Supreme Being (793 reputation)Supreme Being (793 reputation)Supreme Being (793 reputation)Supreme Being (793 reputation)Supreme Being (793 reputation)Supreme Being (793 reputation)Supreme Being (793 reputation)
Group: Forum Members
Posts: 99, Visits: 2.5K
Hi Lee,
Chemical release agents are too slippery to paint a Gell coat or resin on to. What should work is to apply the freecoat as recomended and then apply a coat or two of wax release agent. The wax will adhere to the Freecoat and the resin will adhere to the wax. This is a better release than wax only.

Brian.
Melleen
Melleen
Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)
Group: Forum Members
Posts: 4, Visits: 118
Sorry for the late response everyone... Brian, Thanks for the quick reply... You saved my weekend! I did just as you said and applied the wax after the frekote, and it worked but I had to keep spreading the epoxy until it started to thicken, because if was still fish-eyeing in a few spots.  Hanaldo,I checked my mold release wax and it was silicone free, there is so much to learn! Thanks!!! f1rob, I checked into chemlease but it was not available locally. Warren, Fish-eyeing is not very cool, but I guess this is how you learn.Thanks!! Thanks EVERYONE!! 

Lee Adams

www.melleen.com

info@melleen.com
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Melleen - 11 Years Ago
Brian_s - 11 Years Ago
Melleen - 11 Years Ago
Hanaldo - 11 Years Ago
f1rob - 11 Years Ago
Warren (Staff) - 11 Years Ago
Warren (Staff) - 11 Years Ago
Melleen - 11 Years Ago
Hanaldo - 11 Years Ago
Matt (Staff) - 11 Years Ago
Melleen - 11 Years Ago
Matt (Staff) - 11 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search