1 core layer Lantor SoricXF 3mm. Left 1 layer carbon cloth and right 2 layers on the front side.
Concluded: to lay down 2-3 layers of carbon fiber on the front side in order to avoid the impression.
p.s. weight plates 20x20 cm = 100 grams )  Lightweight and durable )
Infusion without mesh, without peel-ply.



Edited 11 Years Ago by pahanes
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
As I don't know the reason for the test this may be an unfair comment but for a core to add any real strength it needs to have balanced layers of reinforcement either side of it, hence the term core. When there is only reinforcement on one side the stack can delaminate under load.

Warren

Carbon Copies Ltd
pahanes
pahanes
Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)
Group: Forum Members
Posts: 29, Visits: 20K
wozza (02/10/2014)
As I don't know the reason for the test this may be an unfair comment but for a core to add any real strength it needs to have balanced layers of reinforcement either side of it, hence the term core. When there is only reinforcement on one side the stack can delaminate under load.

Warren


Reason for the test - to see whether leaves imprint Soric XF
Edited 11 Years Ago by pahanes
pahanes
pahanes
Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)
Group: Forum Members
Posts: 29, Visits: 20K
Can delaminate... I'm not sure that this can happen. Should be a big load
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
pahanes (02/10/2014)
Can delaminate... I'm not sure that this can happen. Should be a big load



The core is only there to separate the outer layers of reinforcement, in basic terms the thicker the core the stronger the laminate. If there is only reinforcement on one side the core is doing very little to add strength. Thickness but not strength.

Warren

Carbon Copies Ltd
ChrisR
ChrisR
Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)Supreme Being (2.8K reputation)
Group: Forum Members
Posts: 363, Visits: 3K
I think the test was purely to see how many layers you have to put over soric to prevent print through rather than making a panel with just carbon on one side.

You can have unbalanced laminates, it just depends on the forces going through it but then you have to carefully control the cure cycle etc to prevent distortion 
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
ChrisR (02/10/2014)
I think the test was purely to see how many layers you have to put over soric to prevent print through rather than making a panel with just carbon on one side.

You can have unbalanced laminates, it just depends on the forces going through it but then you have to carefully control the cure cycle etc to prevent distortion 



Agreed, and I have done it myselfSmile when the core is there purely to add thickness. But then its not really a core.

Warren

Carbon Copies Ltd
pahanes
pahanes
Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)Supreme Being (297 reputation)
Group: Forum Members
Posts: 29, Visits: 20K
Ok. I do the same on both sides Smile