I have finally got a technic to fill pin holes in one shot that I will share with the group.

1. Sand your part with 220 paper.

2. Wipe down with pure Alcohol not thinner or prime wash or acetone.

3. I have a large needle (4 inches) and have flattened the point just a bit.
    At ninety degrees lightly push the needle into each and every pinhole and twist.
    (this opens and scores the pinhole)

4. Wipe and rub in the alcohol again, very wet, blow dry with high pressure.

5. Mix a small batch of automotive clear and brush on the affected area. (a good thick coat.)

6. Now with a gloved finger rub the clear in with circular motions. (be aggressive)

7.Now brush another coat of clear on right away. Wait 10 minutes and brush on another coat with what you have left over.

8. I then put the part in my hot box at 110 f over night.

9. Flat sand with 220 grit. BANG the pinholes are ALL gone!

10. clear again with your spray equipment and you are ready to wet sand and compound.

NOTE: I have posted this technic because it works. I used to have to go over a part sometimes 4 times to get rid of all of the pinholes.

If you are a professional Auto Body painter this will sound barbaric, but you can't argue with success.

Hope this helps.

Fred






  
Reply
FLD
FLD
Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)
Group: Forum Members
Posts: 468, Visits: 2.7K
I've found that diluting clear down A LOT gets it into the pin holes.  I dilute with equal volume to spray but 2 volumes for pin holes.  I brush this on and really work it in to the pin holes.  3-4 coats like this (30 min dry time) and then I can flat and spray.  I've found no need for the aggresive needling this way.  Its all about sealing the holes IMO.