4" intake pipe


Author
Message
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Hey all,



Thought I would just post up the latest project I have been working on; can always do with being told how to do it better.



So the project is a 4" intake pipe for my R34 Skyline. I wanted to attempt making something from scratch, and given I only had a 3" intake pipe previously I couldn't use that to make a mould for this one. So I started off by using the centreline of my current intake pipe to make a 3D drawing with the dimensions and cross-sections that I needed. I also added 100mm to the straight section on the end, as I wanted to move the air filter further away from the exhaust manifold:













From there I was able to print out the cross-sections I needed, and transfer them to some 3mm balsa wood:

1978698_10151893592392541_851850552_n.jp


Which allowed me to create the skeleton structure of the part:

13258_10151893592592541_220306668_n.jpg

1969113_10151893592482541_2049077103_n.j

I then needed to in-fill the gaps, so I made some low density polyurethane foam using a 2-part pour in place system. With this being the product. I made 4 of these 'blocks'.

1939973_10151864422067541_1752244226_n.j

Then I used this foam to fill in the 'body' of my part:

1800297_10151893592332541_2015330979_n.j

10001515_10151893592277541_1181756648_n.


Trimmed and sanded down to size, and voila!

1002650_10151893592227541_412985007_n.jp

1507560_10151893592162541_1344011204_n.j

From here, I filled and sealed the part with epoxy resin filled with microballoons:

1625670_10151893592107541_491525122_n.jp

1743691_10151893592047541_1909517110_n.j

Then used a stainless steel and fibreglass reinforced body filler to fill in the big gaps:

1896929_10151893591957541_1177675812_n.j

Flattened it down: 

1798764_10151893591882541_853076597_n.jp

10001573_10151893591832541_647456446_n.j

Then used the same filler to cover the whole thing, so I could fill in any low spots in the foam:

1975156_10151893591732541_1009989563_n.j

Sanded it down again, then trial fitted it in the car:

1621730_10151893591622541_381023724_n.jp

1965001_10151893591557541_1479490234_n.j

1907562_10151893591442541_1212210863_n.j

Perfect fitment to the mm!

10006383_10151893591587541_810697348_n.j


Replies
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Well given the surface of the fitting flange is flat, and the pipe is curved, will that not give me two sides where the adhesive will have to do more gap filling? And hence not work so well with the masking tape? 

What if I bonded the fitting in from the inside using the epoxy adhesive as I was planning, and then put 2 carbon strips over the back of it to give it some more surface area and support, and vac bag it. As it's not threaded on its bore, I would then be able to drill out the hole from the carbon? If that makes sense? 
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
Hanaldo (31/03/2014)
Well given the surface of the fitting flange is flat, and the pipe is curved, will that not give me two sides where the adhesive will have to do more gap filling? And hence not work so well with the masking tape? 

What if I bonded the fitting in from the inside using the epoxy adhesive as I was planning, and then put 2 carbon strips over the back of it to give it some more surface area and support, and vac bag it. As it's not threaded on its bore, I would then be able to drill out the hole from the carbon? If that makes sense? 


I shaped the bosses with a Dremmel to match the curve of the tank, that way it is effectively the same as two flat surfaces being bonded together. The lip on the fitting in your link may not be thick enough to do that, not sure. On the second version I modified the mould by bonding in flat discs of Ally where I wanted the fittings. Once infused the part has flat areas moulded in making attaching the fittings easier. Can't see why what you are suggesting won't work, just seems like quite a bit of extra work. If the part is for you then that's not really a problem but for me the extra time would have to be added on to the final cost of the tank.

Warren

Carbon Copies Ltd
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
carbonfibreworks - 11 Years Ago
matthieutje65 - 11 Years Ago
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
Toffee - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
ajb100 - 11 Years Ago
Hanaldo - 11 Years Ago
ajb100 - 11 Years Ago
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
wozza - 11 Years Ago
wildcard - 11 Years Ago
Hanaldo - 11 Years Ago
Hanaldo - 11 Years Ago
wildcard - 11 Years Ago
Hanaldo - 11 Years Ago
wildcard - 11 Years Ago
Hanaldo - 11 Years Ago
wildcard - 11 Years Ago
Nick10 - 11 Years Ago
Hanaldo - 11 Years Ago
asmasm - 11 Years Ago
Hanaldo - 11 Years Ago
Jadleybray - 8 Years Ago