Group: Administrators
Posts: 2.5K,
Visits: 8.5K
|
It is quite common with very slippery release agents such as EasyLease that you get the fisheyeing effect on surfaces, especially sloped surfaces. You have to keep working it until it begins to thicken and gel and stays in place.
If you are really struggling, you can coat the mould in a layer of mould release wax on top of the EasyLease as it will then have a slightly less slippery surface and you will get less fisheyeing.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|