Posts: 32, Visits: 99
So I have done many infusions and they most of the time went ok.
only problem I had was because of heat the parts started getting some rpint though ( bike and car parts)

So I now wanted to post cure my parts in mould so it wont get print through anymore after its clearcoated and put on the bike or car.

I always use IN2 Epoxy Infusion Resin with fast harder or mixed fast and slow.

I got perfect vacuum droptested over night.
after part was infused I had the vacuum on until the resin was gelled up.
Got the part sitting 48H in room temp no signs of air in infusion mesh or anything.
than I had it in my oven for 3H at 40°C 

let it get to room temp and the part has print throug Sad

mould was postcure to 90°C
and stil got mirror finish on it. 


Attachments
Edited 3 Years Ago by kip
Reply
kip
kip
kip
posted 3 Years Ago HOT
Supreme Being (312 reputation)Supreme Being (312 reputation)Supreme Being (312 reputation)Supreme Being (312 reputation)Supreme Being (312 reputation)Supreme Being (312 reputation)Supreme Being (312 reputation)Supreme Being (312 reputation)Supreme Being (312 reputation)
Group: Forum Members
Posts: 32, Visits: 99
Lester Populaire - 12/30/2022 2:17:59 PM
At some point resin will always shrink to a certain degree, and while curing in the mould can reduce print through, the laminate will always have some internal stresses and will relax over time and give you print through. This is a mayor pain in the neck even for big automotive manufacturers, and somewhat worse with loosely controlled processes in a garage.

Thankyou 

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
kip - 3 Years Ago
     Nobody ?
kip - 3 Years Ago
Warren (Staff) - 3 Years Ago
kip - 3 Years Ago
Warren (Staff) - 3 Years Ago
kip - 3 Years Ago
SleepingAwake - 3 Years Ago
             Thankyou
kip - 3 Years Ago
Hanaldo - 2 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search