Best clear coat for carbon fiber panels?


Author
Message
Hanaldo
Hanaldo
Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)Supreme Being (33K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Duratec also offers no UV protection, despite its branding. Ive tested this thoroughly, and concluded that parts are almost better off as raw epoxy than coated with Duratec. They will suffer from UV exposure quicker with Duratec on them (obviously this is true of the epoxy I am using, some epoxies are more sensitive than others). The benefit is that the Duratec can be sanded back and polished again, so you can restore the finish whereas raw epoxy will be ruined.

The best is to do as Fasta suggested, coat with Duratec to avoid any pinholing issues, then report with a top quality automotive 2k for UV protection. Obviously this is the most expensive and the most labour intensive route.
Edited 5 Years Ago by Hanaldo
Fasta
Fasta
Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)
Group: Forum Members
Posts: 468, Visits: 3.5K
vniebles - 3/8/2021 7:44:27 PM
I'm looking at options for clear coating CF+epoxy panels and was wondering what the difference is between a clear coat like Duratec Sunshield and more economical automotive clear coat sprays (like EW 2K High Gloss Aerosol)? 

Duratec is easier to spray thicker for buildup or filling imperfections etc.

Two parts clears are typically thinner and more difficult to fill imperfections quickly.

I find the duratec whilst awesome to use has a downside in that when scratched it seems to leave a very white marking so any damage will show up worse than automotive clears.

You can use duratec like a primer for filling and sanding etc as it works great for this but then also spray finish with automotive two part clear.








Edited 5 Years Ago by Fasta
vniebles
v
Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)Supreme Being (101 reputation)
Group: Forum Members
Posts: 6, Visits: 38
I'm looking at options for clear coating CF+epoxy panels and was wondering what the difference is between a clear coat like Duratec Sunshield and more economical automotive clear coat sprays (like EW 2K High Gloss Aerosol)? 