First Attempt - Results Question


Author
Message
AlpineCoupe
A
Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)
Group: Forum Members
Posts: 45, Visits: 2.1K
This was a practice run at resin infusion. I had never tried it and wanted to see how it went. Overall I learned a lot (mostly what not to do) and this was the result. Panel is 3 plys of 3k 2x2 twill, on a glass table top that was waxed with 5 coats of Partall #2.

I'm wondering if anyone can help identify the cause of the couple of dull spots on the panel. Perhaps the resin didn't penetrate all of the way through? Issue with using just wax? Pinhole leak in the bag?



I tried to grab a slightly more up close shot:


Thanks for the help as always!



Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Yeh looks like a slight release issue, which isn't uncommon with wax on glass. Wax doesn't bond well to glass, so it often isn't a suitable release agent on its own (when used on glass). Ideally you want a chemical release agent.
AlpineCoupe
A
Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)
Group: Forum Members
Posts: 45, Visits: 2.1K
Hanaldo - 1/22/2021 2:03:04 PM
Yeh looks like a slight release issue, which isn't uncommon with wax on glass. Wax doesn't bond well to glass, so it often isn't a suitable release agent on its own (when used on glass). Ideally you want a chemical release agent.

Thanks! I have some 700nc that I'll try instead of the wax. 

Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
700NC should be much more suitable. Just make sure you thoroughly clean the wax off first!
AlpineCoupe
A
Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)
Group: Forum Members
Posts: 45, Visits: 2.1K
Hanaldo - 1/22/2021 11:41:57 PM
700NC should be much more suitable. Just make sure you thoroughly clean the wax off first!

Yep! Going with a degreaser and then an IPA wipe down before I apply the 700nc.


AlpineCoupe
A
Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)Supreme Being (663 reputation)
Group: Forum Members
Posts: 45, Visits: 2.1K
Second attempt worked out much better. Used the 700nc and release was very good. Thanks again for the help!