Post Curing even when 2k clearing?


Author
Message
Warren (Staff)
Warren (Staff)
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
chriscnf - 9/19/2020 8:14:05 AM
Warren (Staff) - 9/18/2020 2:25:44 PM
UV stability and Heat resistance are entirely different and unrelated.

An oven post cure is done usually to maximise the HDT of a part, especially where exposed to higher temperatures so that the part will not go soft when exposed to heat in service.

A UV protective clear coat is an entirely separate process.  The only overlap is if the lacquer also needs a postcure for heat reasons.

Does post cure have a significant effect on strength and stability?

With most room cured resins it does make a noticable difference. Its hard to guestimate but perhaps 20% improvement at best?  Where it does help significantly is with HDT of the cured part. 


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
bennyT
b
Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)
Group: Forum Members
Posts: 11, Visits: 777
Warren (Staff) - 9/18/2020 3:24:24 PM
Yes that is correct

Thanks Warren

chriscnf
c
Supreme Being (502 reputation)Supreme Being (502 reputation)Supreme Being (502 reputation)Supreme Being (502 reputation)Supreme Being (502 reputation)Supreme Being (502 reputation)Supreme Being (502 reputation)Supreme Being (502 reputation)Supreme Being (502 reputation)
Group: Forum Members
Posts: 34, Visits: 2.7K
Warren (Staff) - 9/18/2020 2:25:44 PM
UV stability and Heat resistance are entirely different and unrelated.

An oven post cure is done usually to maximise the HDT of a part, especially where exposed to higher temperatures so that the part will not go soft when exposed to heat in service.

A UV protective clear coat is an entirely separate process.  The only overlap is if the lacquer also needs a postcure for heat reasons.

Does post cure have a significant effect on strength and stability?

Warren (Staff)
Warren (Staff)
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Yes that is correct


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
bennyT
b
Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)
Group: Forum Members
Posts: 11, Visits: 777
Warren (Staff) - 9/18/2020 2:25:44 PM
UV stability and Heat resistance are entirely different and unrelated.

An oven post cure is done usually to maximise the HDT of a part, especially where exposed to higher temperatures so that the part will not go soft when exposed to heat in service.

A UV protective clear coat is an entirely separate process.  The only overlap is if the lacquer also needs a postcure for heat reasons.

Thanks Warren, so am I correct in saying that the heat will cause the softening of the part and the uv rays will more likely cause the part to fade and discolour etc?

Ben
Warren (Staff)
Warren (Staff)
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
UV stability and Heat resistance are entirely different and unrelated.

An oven post cure is done usually to maximise the HDT of a part, especially where exposed to higher temperatures so that the part will not go soft when exposed to heat in service.

A UV protective clear coat is an entirely separate process.  The only overlap is if the lacquer also needs a postcure for heat reasons.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
bennyT
b
Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)Supreme Being (163 reputation)
Group: Forum Members
Posts: 11, Visits: 777
Hey All,

I'm just wondering whether the experts on here post cure their carbon fibre parts that are going to be exposed to UV rays even when they are going to 2K clear the part as well.

As I understand it, both methods will protect carbon fibre from UV exposure and stop the item getting soft in the heat so therefore is there a need to do both? 
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search