Oh dear... This is heartache.
The heat won't be the issue if the gelcoat cured at room temperature. If you accelerated the cure of the gelcoat by applying heat before it cured, then this could mess with the release. But once already cured, the gelcoat can't then bond to the substrate if it is later heated. So I daresay the coating on the pattern was not compatible with the gelcoat and it has reacted and stuck. Either that, or an application issue.
None of that really helps you now, but unfortunately there isn't much you can do now. Heat may help, as polyesters break down quite quickly with heat and you may be able to damage the gelcoat enough to break the bond. Realistically I think brute force is really the only thing that is going to get the part out, so chances are it is going to get pretty damaged in the process.
|