Hello. Sorry for opening a new topic, i have not found a similar issue anywhere else.
The problem occurs when I m mixing the resin with the combined slow and fast hardner. After thorough mixing, some white flakes start to appear in the cup that float arround. If i mix them separately, the mixing is completely clear. I have tried putting the hardners in the cup firstly and mixing them thoroughly before adding the resin, but with no result, everytime the hardners are combined it is like the resin starts coagulating when mixing.
Edited 7 Years Ago by catacls
Replies
Steve Broad
Steve Broad
Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
Where do you live?
catacls
c
Supreme Being (113 reputation)Supreme Being (113 reputation)Supreme Being (113 reputation)Supreme Being (113 reputation)Supreme Being (113 reputation)Supreme Being (113 reputation)Supreme Being (113 reputation)Supreme Being (113 reputation)Supreme Being (113 reputation)
Group: Forum Members
Posts: 10, Visits: 180
Steve Broad - 10/6/2018 11:55:40 AM
Where do you live?

Romania

Steve Broad
Steve Broad
Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)Supreme Being (3.3K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
catacls - 10/6/2018 12:15:15 PM
Steve Broad - 10/6/2018 11:55:40 AM
Where do you live?

Romania

I am just clutching at straws thinking that weather conditions could be a factor.

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
catacls - 7 Years Ago
Matt (Staff) - 7 Years Ago
catacls - 7 Years Ago
catacls - 7 Years Ago
Steve Broad - 7 Years Ago
             Romania
catacls - 7 Years Ago
Steve Broad - 7 Years Ago
catacls - 7 Years Ago
catacls - 7 Years Ago
Steve Broad - 7 Years Ago
catacls - 7 Years Ago
Warren (Staff) - 7 Years Ago
Rich (Staff) - 7 Years Ago
catacls - 7 Years Ago
Warren (Staff) - 7 Years Ago
catacls - 7 Years Ago
Dravis - 7 Years Ago
Warren (Staff) - 7 Years Ago
Steve Broad - 7 Years Ago
                 This parcel wasn t transported by plane.
catacls - 7 Years Ago
Rich (Staff) - 7 Years Ago
Steve Broad - 7 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search