Group: Forum Members
Posts: 10,
Visits: 180
|
Also, I encounter another problem with the resin, so I will post it on this same topic. In combination with the fast hardner, the resin cures rock solid but with a form of amine blush. The surface remains sticky to the touch after curing, which won t be an issue on the surface layer because it can be easily washed with water i noticed, but sanding the component heavy delamination between layers occurs, which requiers the component to be thrown away... I have made a test: in a closed working area with 45% humidity and 23 degrees temp I laminated 3 CF components. 1 with 50/50 fast and slow, 1 with slow and 1 with fast hardner. The 2 components containing fast hardner cured with a very sticky finish and a surface imperfection, and the one with slow hardner cured perfectly. I am running out of options, I don t see what is causing all this issues and I honestly don t believe EL2 is a bad resin, as it didn t get bad feedback from other users.
|