Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)
Group: Forum Members
Posts: 680, Visits: 1.9K
Hi Bob,

OK, that should be OK. If the filler is polyester filler (whcih most of them are) you will need to ensure that the polyester filler is completely cured and is no longer smelling of styrene. If it is, you should wait a while for it to fully cure off and stabilise a bit otherwise you run the risk of the filler upsetting the release agent (whether it's wax or something else).

In terms of your paint finish, it's fine to do this but please make sure you use a two-pack / 2k paint (polyurethane or acryllic) NOT a rattle-can spray paint. We have endless horror stories from customers who have used rattle-can spray paint on their patterns and then have lots of problems releasing moulds.

All the best, Matt

Matt Statham
Easy Composites / Carbon Mods - Technical Sales
bob
bob
Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)
Group: Forum Members
Posts: 2, Visits: 69
Hi Matt
Thanks  ,Its a foam pattern , 2mm chock layer , filler  and  soft sanding . seems has clean surface  ,i can continue put some more  filler for last layer and then sanding ,or painting by color ,i  prefer   paint it by color  for checking the surfaces  Discuss

http://www.talkcomposites.com/Uploads/Images/905d7ba7-cefc-4265-b9ad-037c.jpg
Edited 14 Years Ago by bob
Matt (Staff)
Matt (Staff)
Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)Composites Expert (Staff) (13K reputation)
Group: Forum Members
Posts: 680, Visits: 1.9K
Hi Bob,

Can you give me a little more information on exactly what you've got at the moment (a foam pattern, an MDF buck or just a 3D model)?

Matt

Matt Statham
Easy Composites / Carbon Mods - Technical Sales
bob
bob
Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)Forum Member (42 reputation)
Group: Forum Members
Posts: 2, Visits: 69
DiscussI want be sure my model and mold can be easy seprate from eachother so i am confused about painting my model by color or coat by filler for finishing

http://www.talkcomposites.com/Uploads/Images/905d7ba7-cefc-4265-b9ad-037c.jpg
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search