White spots inside of my Carbon Fiber Epoxy Laminate


Author
Message
fibernoob
fibernoob
Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)
Group: Forum Members
Posts: 34, Visits: 134
tsombnik - 1/9/2018 7:21:08 AM
fibernoob - 1/8/2018 11:58:06 PM
Im not sure its your case... but  I have had similar problems when I used too much (wax based) release agent and did not polish it into the mold.   




Hello fibernoob,
we also used wax based release agent in the area of the sealing cord, so that we can use it again if resin reaches the sealing areas of the tool. So yeah, im pretty sure this can be the reason. We are going to clean the tool again and wont use the wax release agent anymore.
If somebody has another idea though, please tell me BigGrin Maybe it can help.

Thank you for your help!

Nik


After getting some information, i discovered that  wax based release agent has to be applied and thoroughly polished and left for some time for the solvents to evaporate and leave just a thin film of wax (invisible chemical barrier).   Remember that your part will replicate the texture of your mold... if its smooth and well polished (shiny surface) with release agent it will come out perfect.

In my case, I thought that the more release agent i would cover the part with  ... the easier it would demold!   That was my mistake.

The part then showed similar white residues on many places.   Check if those white spots have a similar greasy texture to make sure its release agent.

You can use Water Based release agent (PVA) but it is not as easy to polish or spread uniformly.

If the problem is not release agent related, it can be what the other comments are suggesting.   There are valid points being made... Humidity , Resin Ratios etc.  

Good Luck !


oekmont
oekmont
Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)
Group: Forum Members
Posts: 550, Visits: 27K
what type of pump are you using? what do the specifications say how much pressure it can reach?
30mbar happens to be the boiling point of water at room temperature. If you got a moisture problem, the pressure stops at this point during evacuation. Because of this, I degas at least down to 6mbar, at wich the boiling point is at 0°C. And during infusion, I try to maintain a slightly higher pressure, around 6-7 mbar, to prevent further degassing.

tsombnik
t
Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)
Group: Forum Members
Posts: 6, Visits: 147
oekmont - 1/9/2018 1:08:09 PM
still, there is a vacuum inside the mold, and the resin front is under vacuum. What kind of pump are you using? Are you using the same pump for the evacuation as for the degassing? What negative pressure do you reach?

Ah okay, yes you are correct. We are using the same pump for evac and degassing. We reach a value up to 30 mbar remaining pressure

oekmont
oekmont
Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)
Group: Forum Members
Posts: 550, Visits: 27K
still, there is a vacuum inside the mold, and the resin front is under vacuum. What kind of pump are you using? Are you using the same pump for the evacuation as for the degassing? What negative pressure do you reach?

tsombnik
t
Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)
Group: Forum Members
Posts: 6, Visits: 147
We are not directly doing an infusion. We close the tool, pump out all the air and therefore create a vacuum. Then we have a resin storage which is set under a pressure of 0,7 bar. After the vacuum is created inside the mould, we open the vents and the resin gets pumped into the tool. So we have both, vacuum inside of the mould and the resin gets pumped inside with a pressure of 0,7 bar.
oekmont
oekmont
Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)
Group: Forum Members
Posts: 550, Visits: 27K
during infusion, the outgassing happens where the pressure is the lowest, which is at the flow front. At bridging areas, this gas can accumulate, and stay there during the solidification. This gas consists of trapped air and physically soluted gasses, wich contains h2o. After the impregnation this moisture diffuses back into the resin, but can't get very far.

tsombnik
t
Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)
Group: Forum Members
Posts: 6, Visits: 147
oekmont - 1/9/2018 9:00:26 AM
I've had similar effects caused by moisture. the storage of the resin might be too cold, so that water condense on the resin, once it's in the mixing pot.
Do you degas your resin before the process? This can be a countermeasure against moisture. Additionally the degassing foam wich occurs without pre-degassing might cumulate in bridging areas, and produces this opaque resin after the compression. Do you have the access to a microscope for a mircosection?


Hi oekmont,
yes, we use an Exicator for degasing. Something like this: (https://goo.gl/images/W822mS)
So i guess the degasing foam cant be the reason?
For future experiments we will degas way longer to be sure! Nowadays we only degas for around 5 minutes.
But if you would be right, wouldnt all the resin be opaque, not only in the bridging areas? If you look closely at the bottom of the picture, just below the fibers, you can see the resin of the ring gate being clear.
I dont have access to a microscope. And even if i had, i dont have the skills to see anything Tongue

Edited 8 Years Ago by tsombnik
oekmont
oekmont
Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)Supreme Being (8K reputation)
Group: Forum Members
Posts: 550, Visits: 27K
I've had similar effects caused by moisture. the storage of the resin might be too cold, so that water condense on the resin, once it's in the mixing pot.
Do you degas your resin before the process? This can be a countermeasure against moisture. Additionally the degassing foam wich occurs without pre-degassing might cumulate in bridging areas, and produces this opaque resin after the compression. Do you have the access to a microscope for a mircosection?


tsombnik
t
Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)Forum Guru (65 reputation)
Group: Forum Members
Posts: 6, Visits: 147
fibernoob - 1/8/2018 11:58:06 PM
Im not sure its your case... but  I have had similar problems when I used too much (wax based) release agent and did not polish it into the mold.   




Hello fibernoob,
we also used wax based release agent in the area of the sealing cord, so that we can use it again if resin reaches the sealing areas of the tool. So yeah, im pretty sure this can be the reason. We are going to clean the tool again and wont use the wax release agent anymore.
If somebody has another idea though, please tell me BigGrin Maybe it can help.

Thank you for your help!

Nik

fibernoob
fibernoob
Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)Supreme Being (666 reputation)
Group: Forum Members
Posts: 34, Visits: 134
Im not sure its your case... but  I have had similar problems when I used too much (wax based) release agent and did not polish it into the mold.   




GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search