I suspect you have moved up to a finer grit too soon or you have got a bit of grit in your paper. Zoomed in you can see a lot of scratches on the surface. The solution is to go back down the grits until you can remove the scratches then work back up to 1200-1500 and then polish again. Hopefully that should solve the problem.