By LioH - 12/8/2017 12:39:04 PM
Hi, We finally finished our BMW 3-series interior in carbon. We followed step by step the tutorial but we have in thing really strange. Left door handle is super shiny extreme deep gloss, near-perfect gloss but the right one is not so gloss, not matte but I don't have that super shiny effect. The piece looks a bit blury and we restarted the sanding process 2 times and the first time wasn't correct enough. (From 400, 800, 1200 + polish).
We have done the same process for both piece. What can it be ? I need you advice. Thanks, Lionel

|
By Warren (Staff) - 12/8/2017 1:21:06 PM
I suspect you have moved up to a finer grit too soon or you have got a bit of grit in your paper. Zoomed in you can see a lot of scratches on the surface. The solution is to go back down the grits until you can remove the scratches then work back up to 1200-1500 and then polish again. Hopefully that should solve the problem.
|
|