You dont need to have fancy workshops if you are determined enough to make some carbon parts for your car.

All this was done in my lounge.

Lay up the carbon in the top skin mould:


used 2 layers of carbon with a foam core.

Bag it up and start to infuse:


all done:


debag and take off the peel ply and mesh:


Pull it out the mould and see the finished top skin:


get your inner frame mould prepped:


Lay in the carbon:

added 2 layers of kevlar in and around the hinge area to prevent it coming to pieces in a crash

Add the peel ply, mesh and bag it up:



And infuse the part:



debag it and strip off the peel ply:

the frame popped out of the mould while tugging off the peel ply!

Detail in the hard to do corners came out good.

bonded in the captive nuts for the hinges.

Trim both parts and lay the top skin back in the mould:



bond together the top part and inner frame using polyurethane adhesive, then use conveniently found weights from the kitchen to press the two parts together.

Doing it in the top skin bonnet means the bonnet maintains the correct shape and you dont get any warping.

And the finished bonnet.

Preferably take photos where you wont get wierd reflections!!!

Final part came in at 4kg.
pk_090
pk_090
Supreme Being (383 reputation)Supreme Being (383 reputation)Supreme Being (383 reputation)Supreme Being (383 reputation)Supreme Being (383 reputation)Supreme Being (383 reputation)Supreme Being (383 reputation)Supreme Being (383 reputation)Supreme Being (383 reputation)
Group: Forum Members
Posts: 47, Visits: 169
Your Mrs, must be very understanding Warren!
Looks like a cracking final part!
FLD
FLD
Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)
Group: Forum Members
Posts: 468, Visits: 2.7K
Thats awesome!  Is that a 200g layer core then 200g?  The reason I ask is that I'm considering similar and I'm interested in the rigidity.  I was contemplating 200g (for nice finish) 600g, core, 600g, 200g. 
CarbonMike
CarbonMike
Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)
Group: Forum Members
Posts: 31, Visits: 45
Bloody hell you mustve been as high as a kite lol

Good job though, Puma bonnet is it? Certainly looks like one to me.

Just to add, you wouldve saved a small fortune, and probably a whole lot of heavy lifting by making the mould from fibreglass as oppose tooling putty!
Edited 13 Years Ago by CarbonMike
Warren
Warren
Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)
Group: Administrators
Posts: 214, Visits: 782
the skin is just 200g carbon, 2mm soric then 200g carbon.

Perfectly stiff enough as a skin on a framed panel like that.

Wasnt high at all.  Remember epoxys are low odour.


Didnt use mould making putty. Used fibreglass, coremat and carbon in the moulds.
Edited 13 Years Ago by Warren
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
Isn't epoxy more harmful than polyester because it has a low odour and you don't smell it? Smile
OT great work Smooooth

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




Edited 13 Years Ago by matthieutje65
CarbonMike
CarbonMike
Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)
Group: Forum Members
Posts: 31, Visits: 45
Warren (04/07/2012)
the skin is just 200g carbon, 2mm soric then 200g carbon.

Perfectly stiff enough as a skin on a framed panel like that.

Wasnt high at all.  Remember epoxys are low odour.
Didnt use mould making putty. Used fibreglass, coremat and carbon in the moulds.


Ah right I see, the mould looks like its made from an EC/CarbonModz tooling gel coat/mould putty. The "being high as a kite" comment was actually sarcasm but oh well.

matthieutje65 (05/07/2012)
Isn't epoxy more harmful than polyester because it has a low odour and you don't smell it? Smile

OT great work Smooooth
 
Cant really comment on which is more harmful as its not my area of expertise. But any resin with high amounts of Thixothorpe (spelling?) and Phennol will do your respiratory tract some significant harm over time if used in unventilated areas. More so once its cured & being sanded down/cut/grinding etc.
Edited 13 Years Ago by CarbonMike
Warren
Warren
Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)
Group: Administrators
Posts: 214, Visits: 782
i use the tooling gel coat.
CarbonMike
CarbonMike
Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)Supreme Being (221 reputation)
Group: Forum Members
Posts: 31, Visits: 45
Warren (06/07/2012)
i use the tooling gel coat.


I knew I recognised that shade of green BigGrin
Carbon Tuner
Carbon Tuner
Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)
Group: Forum Members
Posts: 104, Visits: 422
I like it'

I am looking to make a big part soon that has a top and bottom, still I like making the table style molds cause I can make it a square, I hate trying to cut angled baggin film.



If Brute Force Isn''''t working your not using enough...
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search