Metal inserts - Carbon fiber layup


Author
Message
FLD
FLD
Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)
Group: Forum Members
Posts: 468, Visits: 2.7K
Hanaldo (13/09/2015)
How thick a piece of metal are you using? I always think of sheet metal as being like 0.5 to 3mm thick, which isn't really enough for fasteners... Depends what loads the fastener sees, but the rule of thumb is you need at least 4 turns of thread for the fastener to be doing anything. 

I wouldn't be using anything less than 10mm.


The last one was a hard 4.5mm piece of alloy for an M4 thread.  Seems to have held up OK for the last year although it's not supporting anything massive, just a small header tank.
scottracing
scottracing
Supreme Being (5.5K reputation)Supreme Being (5.5K reputation)Supreme Being (5.5K reputation)Supreme Being (5.5K reputation)Supreme Being (5.5K reputation)Supreme Being (5.5K reputation)Supreme Being (5.5K reputation)Supreme Being (5.5K reputation)Supreme Being (5.5K reputation)
Group: Forum Members
Posts: 460, Visits: 5.2K
Apart from when ive been laying up prepreg tooling ive never put inserts into the laminate stack. Its always been the case to cold bond in inserts after the composite has cured and usually post cured. A decent structural adhesive will create a bond that will not fail before the laminate, but you must ensure that the metallic insert is properly abraded and cleaned afterwards, the same with the composite. 
This also allows you to place the inserts in the correct place as they can move about when you place them in the layup.
if you do want to place them in the correct place then use nylon dowel to keep them in place.
Dravis
Dravis
Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
Well .. thickness of the metal insert with relation to the strength of the fastening depends entirely on what size of threading you use.

There are very good resources for calculating the force you can apply to such and such a length of threading of a certain size .. the "ballpark rule" of at least four turns of a given thread is probably not far off for high tensile materials like Hard aerospace alu alloys, steel and titanium..  Bear in mind that the tightening torque of the nuts and bolts SUBTRACT from the available strength... this is also given in various tables, some of which can be found on the internet.  A lot of people seem to forget that tightening the nuts and bolts do NOT make for a stronger "joint"  It just helps to keep the bolt from undoing..

The force that a given thread can hold also depends very much on the thread tolerances, and proper sizing of the holes that you thread.  Too small a hole drilled in Titanium WILL break your tap, even slightly too large a hole drilled in aluminium will produce a weak thread.

The rule I've learned is: for softer alloys the thickness of the fastener has to be twice the drill size for the thread (for standard Metric threads)  Metric Fine and UNF / UNEF can go down to 1 - 1,5 x for thickness.
For harder alloys the rule says:  1:1  i.e. : 5mm Metric requires 4,2 mm thickness to keep the inherent strength.

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
Hanaldo
Hanaldo
Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
How thick a piece of metal are you using? I always think of sheet metal as being like 0.5 to 3mm thick, which isn't really enough for fasteners... Depends what loads the fastener sees, but the rule of thumb is you need at least 4 turns of thread for the fastener to be doing anything. 

I wouldn't be using anything less than 10mm.
FLD
FLD
Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)Supreme Being (5.2K reputation)
Group: Forum Members
Posts: 468, Visits: 2.7K
In the past I've scored the surface of some small bits of sheet metal and then put that in the stack.  Once cured I drill and tap into the piece of sheet.  How effective the scores are for the resin I'm not sure but I had no problems.  This way you don't need to be ultra accurate with your insert placement.
Dravis
Dravis
Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)Supreme Being (7.2K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
I have actually conducted several tests of bonding in and laminating in metal fasteners (made from Grade 5 titanium) for a small shipyard that builds CF pre-fab parts for medium sized vessels.

I can tell you that there is a very small advantage in strength of the fasteners binding to the actual part, from laminating it inside (vac-bag) or infusing it into the CF laminate.  It is simply only cost effective in terms of the work you need to put into it, unless you need to produce a fair amount of copies of the same part.

Bonding the fasteners in with patches of cf fabric laminated on top retains 90 -95 % of the strength of an "infused in" fastener.

Bonding in a simple standard nut will not be very strong, its much better to have some threaded inserts made, that have a larger surface area to bond to and to spread the load over a larger area of the cf laminate.

I can give an example:   an M5 threaded insert machined as a flat disc 18 mm in diameter has more than 600% higher strength, compared to a standard M5 nut laminated into the CF sheet.

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
VVS
VVS
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Moderators
Posts: 226, Visits: 334
I should think the insert I'm the picture is fitted after.

the cf would be drilled and then the insert is actually loose fitted and then crimped with a tool similar to a press stud used in the clothes industry.

Similar fixings are used on the motorcycle industry to put fixings into ally frames, swing arms etc.
Trace Elliott
Trace Elliott
Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)
Group: Forum Members
Posts: 4, Visits: 30
Thanks for the tips, that's really helpful!

I understand how to position the insert, what I don't get is how the fibers manage to go around it.
In the attached picture, is the stack perforated before putting the insert in the hole, or do the fibers go around the insert?
(There's a chance this particular part was drilled and the nut glued, I'm not sure.)
How could I achieve this kind of result by infusion the insert in the laminate?







http://www.talkcomposites.com/Uploads/Images/9a0f0f30-c79c-4a1d-aa92-6113.jpg
Warren (Staff)
Warren (Staff)
Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
There is no set way to do it as it varies with design.  ideally on a straight forward sheet you would need to consider the load direction and place the metal plate such that the load is spread over as much carbon as possible.  Often this is why they are fine to bond on afterwards. 

Positioning is the hard part as you rightly say it would be necessary to locate it somehow so it cannot move during the laminating process. If the nut is sticking out into the mould surface, then a simple recess for the nut would stop it moving. Or you could fabricate a piece of strip to go across the mould which is bolted or secured firmly in a set place. You can then have pre-drilled holes for you to put a bolt into then wind it into the insert thread. Thus the inserts are held in place by bolt and in turn the strip. 

Plenty of other ways with a bit of imagination and design specific to your mould. However in all cases ensure that any mechanism to hold the insert doesn't interfere with the bagging stack.  Most "off the shelf" inserts will have a perforated load spreading plate for better bond which will usually be fine as there is a route for infusion resin to flow.

Also consider using wax to seal the thread of the insert so it is not blocked with resin during the process.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Trace Elliott
Trace Elliott
Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)Supreme Being (106 reputation)
Group: Forum Members
Posts: 4, Visits: 30
Hello everyone,

I'm designing a drone, and I would like to be able to bolt two plates together (rather than use an adhesive, because if something breaks, I'd prefer to be able to change the piece that broke, rather than a whole assembly).
The plates would be 2-3mm thick, made by resin infusion.
To that effect (bolting plates together), I'd like to put a metallic insert in the lamination, prior to the infusion.
The insert would be a nut, essentially.
I know you can make the plate, then drill a hole and glue the insert, but I'd rather infuse the whole thing at once, if it's possible.

My question is: how do you put an insert in the fiber stack?
I read everywhere that you should have pins in the mould to accurately locate the inserts, but very little info on how to blend the insert in the fiber stack.

Should I spread the fibers apart? I'm thinking that won't look good
Should I punch a hole through the stack? Hello fibers everywhere...
Should I lay the first cloth and spread the others around the insert, and grind the first layer to reveal the insert?

If you have any ideas, please do tell :-)

Thank you very much!
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search