primoz1111
primoz1111
posted 11 Years Ago
ANSWER
HOT
Topic Details
Group: Forum Members
Posts: 3,
Visits: 31
Hello!
First hi to everyone using this forum, you got nice community here.
Ok
the PROBLEM
I am using 245 2x2 twill 43% resin rich
prepreg
. As you can see the resin in not equally spread through surface.
My product demands 2 layers of prepreg so when i stack the layers i turn the the sides with more resin facing each other then i combine them so the most resin is in the middle of fibres letting the vacuum do its job.
When i vacuume the prepreg i use release film perforated and breather all stuck in vacuumbag.
My tactic is 3h of vacuuming on room temp then 1-2h on 45C, 1h on 60C and 1h on 70C after that i cure it at 120C for another hour more
This is my BEST result :
So here is the problem why is here areas of pinhole free surface and with pinholes is it the resin not evenly spread the or the problem is my tactic of vacuuming any tips or help will be nice.
P.S. I am using
http://shop1.r-g.
de
/item/390102S vacuum pump
Tags
pinhole
pinhole free
prepreg
Edited
11 Years Ago by
primoz1111
Reply
Like
18
Reply
fgayford
fgayford
posted 11 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 433,
Visits: 1.2K
primoz1111 (17/04/2015)
Hello!
First hi to everyone using this forum, you got nice community here.
Ok
the PROBLEM
I am using 245 2x2 twill 43% resin rich
prepreg
. As you can see the resin in not equally spread through surface.
My product demands 2 layers of prepreg so when i stack the layers i turn the the sides with more resin facing each other then i combine them so the most resin is in the middle of fibres letting the vacuum do its job.
When i vacuume the prepreg i use release film perforated and breather all stuck in vacuumbag.
My tactic is 3h of vacuuming on room temp then 1-2h on 45C, 1h on 60C and 1h on 70C after that i cure it at 120C for another hour more
This is my BEST result :
So here is the problem why is here areas of pinhole free surface and with pinholes is it the resin not evenly spread the or the problem is my tactic of vacuuming any tips or help will be nice.
P.S. I am using
http://shop1.r-g.
de
/item/390102S vacuum pump
First, Do not use perforated film, use non-perforated film. You are bleeding away the resin rather than letting it flow. Also I would not ramp that slow. Just go straight to your cure temperature, so as to allow the resin to reach its lowest viscosity and flow, before it starts to crosslink. (cure).
Hope this helps.
Fred
Reply
Like
14
GO
Merge Selected
Merge into selected topic...
Merge into merge target...
Merge into a specific topic ID...
Open Merge
Threaded View
Threaded View
Pinhole uneven surface
primoz1111
-
11 Years Ago
I'm getting the same surface finish when I vac bag my wet layup. The effect (on both our items)...
amgrace
-
11 Years Ago
I have no problem with sealing. My vacuum stays if i stop the pump but i use pump all the time...
primoz1111
-
11 Years Ago
Hi guys, Can you give the technical data sheet of your prepreg ? 2 reasons that may resolve your...
Julien
-
11 Years Ago
You need to get a proper Out of Autoclave pre-preg to be honest. This part is only 2 layers thick...
morepower
-
11 Years Ago
You say you are using a perforated release film?! must be an unperforated one! ratio fabric/resin is...
matthieutje65
-
11 Years Ago
I never used pre-preg but looking a lot of video, as Matt said right, they use only unperforeted...
Jacopo Carbonio
-
11 Years Ago
[quote][b]primoz1111 (17/04/2015)[/b][hr] Hello! First hi to everyone using this forum, you got...
fgayford
-
11 Years Ago
Hello! Tnx for all replays. It was help full ALLOT!!! i did it no pinholes at all i cant be...
primoz1111
-
11 Years Ago
[quote][b]primoz1111 (22/04/2015)[/b][hr] Hello! Tnx for all replays. It was help full...
creator
-
11 Years Ago
Post Reply
Like
18
Similar Topics
Post Quoted Reply
Reading This Topic
Login
Login
Remember Me
Reset Password
Resend Validation Email
Login
Facebook
Google
Explore
Messages
Mentions
Search