Can someone explain how a resin brake works? the theory behind it and how to make it?

i've seen it mentioned on another forum.

I think the idea is to slow down the infusion process?
Paul (Staff)
Paul (Staff)
Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)
Group: Administrators
Posts: 134, Visits: 614
To be honest many people have there own definitions for a lot of composites terminology, These are the most likely:

Resin break (not brake) between the part and vacuum take off; this is an area between the vacuum distribution (mesh or spiral) and the part itself, the gap between does not contain any flow media mesh and is intended to slow the flow of resin so that the 'advance' of the resin will completly cover the part before getting to the vacuum distribution.

Resin brake (braking) to restrict the flow of resin into the part by partially closing the resin feed line with a clamp, this can help on thicker laminates to prevent the flow media side of the part advancing too far beyond the lower layers in the stack, which can lead to dry areas and pinholes.

If anyone else has any ideas for its meaning, or needs this, or some other terminology explaining, I look forward to hearing from you.

Paul Statham
Easy Composites / Carbon Mods - Technical
Edited 14 Years Ago by Paul (Staff)
MAVERICK
MAVERICK
Supreme Being (417 reputation)Supreme Being (417 reputation)Supreme Being (417 reputation)Supreme Being (417 reputation)Supreme Being (417 reputation)Supreme Being (417 reputation)Supreme Being (417 reputation)Supreme Being (417 reputation)Supreme Being (417 reputation)
Group: Forum Members
Posts: 27, Visits: 39
The way I have seen the breaks done which seems neat was to run the vac spiral about an inch outside of any of the reinforcement, mesh, peel ply etc. the just connect the spiral to the laminate every few inches or so with a 1 inch peice of breather... here's a pic I found, these guys are using choppy mat where I said breather... don't suppose it matters really.

http://www.swallowboats.co.uk/images/stories/swallowboats/storm17/infusion/DSCF5536.JPG

That's also monster spiral... it is a big looking boat I suppose! hope this gives you an idea of what it's about anyway Smile
Carbon Tuner
Carbon Tuner
Supreme Being (1.7K reputation)Supreme Being (1.7K reputation)Supreme Being (1.7K reputation)Supreme Being (1.7K reputation)Supreme Being (1.7K reputation)Supreme Being (1.7K reputation)Supreme Being (1.7K reputation)Supreme Being (1.7K reputation)Supreme Being (1.7K reputation)
Group: Forum Members
Posts: 104, Visits: 422
Yes I saw the need for resin flow manipulation yesterday. this Idea just dawned on me making my latest part. I had the infusion mesh on my part then up on the surface of the mold top. I need to notch the infusion mesh up on top so the resin is forced to flow through the part itself, not directly to the vacuum side.

 

Here's a Pic of What I mean, Next time I'll actuall make the cut. The resin did flow right but still coulda been better.

http://www.carbontuner.com/talk/l3.png



If Brute Force Isn''''t working your not using enough...
Edited 14 Years Ago by Carbon Tuner
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search