Epoxy tooling gel coat


Author
Message
Dravis
Dravis
Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
I've found the EC coating resin to be very good, even if a little expensive... I ad a little bit of graphite powder to thicken it slightly.  It makes a very hard and polishable surface on a plug, i normally wet sand it down to 1200 and polish it with polish and wax.

I've also very successfully used normal laminating epoxy with some filler and dye added ..  (micro glass balloons, graphite  and fumed silica)  The dye makes it easier to spot if you sand through to the next layer


 

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
aza993a
aza993a
Supreme Being (154 reputation)Supreme Being (154 reputation)Supreme Being (154 reputation)Supreme Being (154 reputation)Supreme Being (154 reputation)Supreme Being (154 reputation)Supreme Being (154 reputation)Supreme Being (154 reputation)Supreme Being (154 reputation)
Group: Forum Members
Posts: 10, Visits: 91
I'm guessing you're using it to coat something and desire it to lay flat to give a regular surface, say plug production or surfacing a tool. And not using it to capture the surface of a plug, as the surface detail would be replicated and thus the regularity in the surface not an issue.  Try using a less thixotropic resin or adding in a wetting agent to decrease the surface tension. I've tried a number of wetting agents and a very smooth flat surface can be achieved on the surface of a plug simply by brushing on a regular epoxy treated with a dry wax teflon out of a spray can at 1-2%.
brainfart
brainfart
Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)
Group: Forum Members
Posts: 198, Visits: 1.4K
A flame produces lots of carbon dioxide and water vapour. Not good with amines. I'd rather use a hairdryer or heat gun.
Blackrat
Blackrat
Supreme Being (280 reputation)Supreme Being (280 reputation)Supreme Being (280 reputation)Supreme Being (280 reputation)Supreme Being (280 reputation)Supreme Being (280 reputation)Supreme Being (280 reputation)Supreme Being (280 reputation)Supreme Being (280 reputation)
Group: Forum Members
Posts: 20, Visits: 85
why put it on smoother ? dont see that its going to make a difference ?  what you can try is to warm it up a little and mix smaller quantities at a time
 

also , try running a blow torch over the first layer of toolcoat to pop any bubbles BigGrin
FLD
FLD
Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)
Group: Forum Members
Posts: 468, Visits: 2.7K
Wow!  That is some plug, I'll bet there's a few hours work in that.  I completely agree with your choice of epoxy if you're near your house.  Polyester does smell rather.  I always try to be outside when I use it.
Martin Fraser
Martin Fraser
Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)
Group: Forum Members
Posts: 11, Visits: 148
Hi FLD,

Yeah, the plug is glassed and epoxied (see attached) but another reason for using epoxy is that my workshop is attached to the house and polyester is just so smelly! 

The model is a 1/8th scale of a Westland Wessex Mk1 - 6ft from nose to tail. going for electric on this one but may go turbine on the Mk5 version.

Cheers, Marty
Attachments
Plug glossed.jpg (1.1K views, 88.00 KB)
Edited 12 Years Ago by Martin Fraser
FLD
FLD
Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)
Group: Forum Members
Posts: 468, Visits: 2.7K
The issue with foam and polyester is down to the styrene melting the foam if its the wrong type.  You can seal the foam with a coat of epoxy or use the right foam.  For example I have recently made some wing mirrors.  I used a non-stable foam and coated it with epoxy.  I took moulds from this in polyester gelcoat.  I then made mouldings in carbon / epoxy from the polyester mould.  I see no reason for concern.    However, if you really want to use epoxy then try putting it on thick and you should be fine as its the surface next to the plug that matters.  Alternatively you can wait for it to start to thicken and then smooth it out as it gels.  Out of interest whats your model?  I'm currently building a gas turbine.

ETA:  Been away anywhere nice?
Edited 12 Years Ago by FLD
Martin Fraser
Martin Fraser
Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)Supreme Being (291 reputation)
Group: Forum Members
Posts: 11, Visits: 148
Hi folks, 

Apologies for the late reply - been away.

I've been advised not to use polyester for the moulds as the plug is made from foam and may suffer if it gets too hot and I'm building the finished model using epoxy, GF and carbon.  The tooling gel coat is Easy Composites  https://www.easycomposites.co.uk/epoxy-tooling-gel-coat

Maybe a synthetic brush might put it on smoother?

Thanks for your input guys, Marty
kidpaint
kidpaint
Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)
Group: Forum Members
Posts: 99, Visits: 676
what epoxy tooling gel coat are you using?
FLD
FLD
Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)
Group: Forum Members
Posts: 468, Visits: 2.7K
I wouldn't recomend it.  Can I ask why you need to use epoxy tooling gel?  I currently use polyester tooling gel and I find that cures to a nice, hard, polishable surface. This stuff.  I use it for all laminates without problems.
Edited 12 Years Ago by FLD