Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)Technical Support (2.2K reputation)
Group: Administrators
Posts: 134, Visits: 614
Hi Francois,

Fast-cast is very low viscosity @ 50-60 mPa.s, the lower viscosity epoxy resins such as the IN2 is 225 mPa.s, however this is still very pourable and it works very well for smaller castings, and obviously offers much higher mechanical performance. In you application I'm sure that it would work very well, I would advise using the slower hardener speed as this will reduce the exotherm and result in a more dimensionally accurate final component.

Any fibre reinforcement that you can include into the casting will improve the strength greatly, also as the part has a thread I would also mix graphite powder into the resin as this is excellent at reducing friction and wear.


Paul Statham
Easy Composites / Carbon Mods - Technical
Francois Moal
Francois Moal
Forum Member (25 reputation)Forum Member (25 reputation)Forum Member (25 reputation)Forum Member (25 reputation)Forum Member (25 reputation)Forum Member (25 reputation)Forum Member (25 reputation)Forum Member (25 reputation)Forum Member (25 reputation)
Group: Awaiting Activation
Posts: 1, Visits: 2
Good morning
I need to mould some connection pieces for attaching a rotary brush to a water fed pole. I will use the carbon fibre sleeves to reinforce, but have no experience of the type of resin needed to achieve the best strength. I have done a test with Fast Cast and a thin polyester mat, and it seems successful. Fast Cast is quite liquid, and I find that useful. Would an epoxy still have the same, or approximately the same viscosity? The connectors have coarse threads.
Thank you in advance
Francois Moal
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search