Mould Making
»
Gel Coat with not enough hardener
Gel Coat with not enough hardener
Post Reply
Like
5
Gel Coat with not enough hardener
View
Flat Ascending
Flat Descending
Threaded
Options
Subscribe to topic
Print This Topic
Goto Topics Forum
Author
Message
fgayford
fgayford
posted 12 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 433,
Visits: 1.2K
Jozi (27/08/2013)
I had to make a few tiny repairs to my mould and mixed up such a small quantity of gelcoat I couldn't measure it properly. Mixing it 10:1 I had about 7-8gr of gelcoat and I added a bit of hardener that was less than 1gr, but I'm not sure by how much. I just had a look at the gelcoat 18hrs later and part of it is hard but some of it feels a bit greasy and smears a little on to my finger when rubbed. Will it harden out eventually and if so how long could it take?
If this is polyester resin just apply some steady heat to it and it should cure fine. If the gelcoat doesn't have airdry (we call it) it will stay tack on the surface
Hope this helps.
Fred
Reply
Like
4
H4RTM4N
H4RTM4N
posted 12 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 7,
Visits: 203
I'm affraid I'll have the same problem.
Today I made some repairs on a mould I prepared last week. In addition to the usual gelcoat + MEKP, I added some liquid paraffin (1-2%) to prevent the gelcoat from staying tacky.
After 4h, the gelcoat is way less tacky than usual but it's still 'green'. In case it stays this way, is it possible to make it fully cure so it can be sanded and polished? Would I need to put some tape on it?
Thanks!
Reply
Like
5
Jozi
Jozi
posted 12 Years Ago
ANSWER
HOT
Topic Details
Group: Forum Members
Posts: 18,
Visits: 60
I had to make a few tiny repairs to my mould and mixed up such a small quantity of gelcoat I couldn't measure it properly. Mixing it 10:1 I had about 7-8gr of gelcoat and I added a bit of hardener that was less than 1gr, but I'm not sure by how much. I just had a look at the gelcoat 18hrs later and part of it is hard but some of it feels a bit greasy and smears a little on to my finger when rubbed. Will it harden out eventually and if so how long could it take?
Reply
Like
5
GO
Merge Selected
Merge into selected topic...
Merge into merge target...
Merge into a specific topic ID...
Open Merge
Post Reply
Like
5
Similar Topics
Post Quoted Reply
Reading This Topic
Login
Login
Remember Me
Reset Password
Resend Validation Email
Login
Facebook
Google
Explore
Messages
Mentions
Search