Hey there,

I recently (today) demolded my first mold made using UniMold system (today). It turned out good.

I wanted to point some things people (especially newcomers) would want to know before they start working with it.

Facts:

Room T°: 19°C;

Gelcoat: 1 layer applied with brush; close to 1mm thick; 2% catalyst; time: 1 beer.

Coupling coat: 1 layer of 150 g/sqm; 2% catalyst; time: 1 beer but a bigger one.

Reinforcement: 5 layers of 450g/sqm;  2% catalyst; time: 2.5 hours (and no time for a beer).

Area of the plug: about 1sqm, many curves.

What I learned:

Applying the gelcoat and coupling coat was flawless.

But once I started the reinforcement side, it was another story. It all went good till third coat (on the 5 total). When beginning the third coat, i noticed the faster and faster time of resin gelling on the part.  Yup, it was time for me to hurry (or reduce catalyst amount and/or room temp). Remember I used 2% catalyst and part has a "complex" shape which took time to wetout. I did not reduce catalyst amount, cos "Work in the morning and demold at night" is my moto.

Lucky me, and thats what i wanted to point for new users (or wanna-go-too-fast-guys like me): i really think bristle roller between each coat saved my mold integrity. Some would roll their mold after all the coats, some after 2 layers (i usually do that with non-filled resins), but keep in mind Unimold uses filled resin, which appears to me to be more difficult to "degas" and several layers of 450g/sqm mat dont help.

And yeah, dumb people like me have a god: it all went fine, finally. Final mold temperature was not at all excessive, even with 5 coats of mat and 2% catalyst. Unimold is a great process, I cant wait for my next mold. I hope this topic could help newcomers.

 



 


    A $1000 electronic device will always protect a 10 cents fuse
Edited 13 Years Ago by Joe
Reply
Daz
Daz
Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)Supreme Being (690 reputation)
Group: Forum Members
Posts: 93, Visits: 651
Same happend to me i wish i had had some one there to help as it was a car roof mould

Thought i would have had plentyu of time but as the layers built up so did the heat

Next time i will use less and less catalys as i build up the layers and see how that turns out Unsure