Pleased to report that with helpful advice from your tech team and some forum members I have now successfully made up 6 flat c/f panels in 195 gsm varying from rectangular 400 x 400 mm to triangular 2200 x 450mm by resin infusion. All have eventually come out without voids (yipee), there was some scrap. They only worked well once I heated the layup table to 22c, and heated the resin as it flowed with a hot air gun. I did use a lot more resin than in your tables, but the surplus came off in the peel ply. My panels are 0.35mm thick.

Now can you you help me with sticking these on my grp boat?  I have coarse sanded all the grp, 80 grit. I cannot control the temperature which is ambient in a big steel shed, currently 3c and 65% humididty. I therefore cannot use epoxy the glue them down, because any minor  uneven heating / cooling causes ripples, I have tried. The surface is compound curve, just, but I have formed the panels dry, by heating them till flexible and taping them down to cool. (It works!) I favour using pu 18 adhesive as it is flexible and waterproof, but how on earth do I get an even thicknes of such a thick sticky adhesive over such a big area??? and how do I keep the panels even on top of the adhesive?? Any advice and or clues would be greatly appreciated.
Replies
ezsailor
ezsailor
Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)
Group: Forum Members
Posts: 20, Visits: 75
Iv'e been away for a couple of days as well. Thanks for the reply. Flexing is fairly small in terms of twist, probably less than 2mm in 500. But downwards deflection could be as much as 10mm in the 300 mm between the deck ribs, if you accidentally stand on it (easily done)  I see what you are saying about uneven resin thickness though. I tried epoxy resin with and without filler powder, seemed not to make a difference. Got two on perfect, and four were awful next morning. I was lucky to go very early and managed to rip them off before they were properly cured.

I thought of PU18 because I am familiar with sicoflex, and know you can spread that with an adhesive comb to a fairly even coat, while leaving some thickness to take up very small imperfections in the substrate. Supreme being says it can be combed, and if I smooth it down with a 500mm  long board with layers of soft cloth on the edge (which must help to even it out) and then vac it down do you think I would get better control over it? I could try the smallest piece first. I have to get this right now, the other guys in my club already think I am some sort of magician.
ezsailor
ezsailor
Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)Supreme Being (304 reputation)
Group: Forum Members
Posts: 20, Visits: 75
PS Actually Matt I think what's causing the ripples/big air bubbles is the lack of initial grab that epoxy suffers from. Where they appeared could be clearly seen on the underside  when the sheet was removed, lots of tiny pointed peaks where the bubbles were, and clear combed flat lines where it gripped. Does PU18 have better initial grab?  Using vac to hold down will help to overcome this premature release? Thanks.