Generally degassing is not needed for wet lay up. You can leave the pot to stand for 5 minutes or so. Then use it and waft a heat gun over gently if you have bubbles still there. However, degassing can be done if you have the equipment, and although some air may get in when brushing, it may help a bit.
Also check your mixing method, generally a "folding" type action traps less air as opposed to other stirring methods.
Another factor is temperature. if you are working much below 20C, the resin thickens which means it will trap more air during mixing.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|