Hi. I have had a bit of a disaster, that actually turned out to be a bit of a godsend.

Anyway, My passenger door is fibreglass but I have cut out most of it leaving just the edges to which I plan to stick carbon fibre panels. Did the cutting and made the panels, so far so good.

Sanded the carbon with 80 grit and cleaned with acetone and allowed to dry. Likewise the fibreglass.

Spread on the VM100 and clamped the panels on, one at a time, and left overnight to cure.

All looked Hunky Dory. Offered door up to the opening and discovered that is had twisted! Bugger, now how the hell do I get the carbon panels off? Turned out to be very easy as they just peeled off!

Question is, what dId I do wrong? Photos show edge of panel, I simply scraped off the glue residue with a Stanley blade. The glue is very securely adhered to the fibreglass.





Reply
Steve Broad
Steve Broad
Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
Warren (Staff) - 5/13/2020 11:53:05 AM
Looks like for some reason it didn't grip the carbon. How was the carbon sheet made?

I wonder if it was just the mechanism of peel?  Structural adhesives are vulnerable to peel - you will see some "anti-peel" fixings on bonded structures (eg lotus elise tub). That and the fact the adhesive wasn't cured fully cured might have made it easier to peel.  

Hi Warren
It had been on for over 24 hours. I have since tried again after cleaning with thinners and then acetone and it seems to have worked this time. I guess that there was some sort of residue on the carbon that I didn't get off first time.

Sheet made using prepreg on aluminium mould, release film and breather cloth at 120 deg C

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Steve Broad - 5 Years Ago
Warren (Staff) - 5 Years Ago
Steve Broad - 5 Years Ago
Hanaldo - 5 Years Ago
Steve Broad - 5 Years Ago
Warren (Staff) - 5 Years Ago
Steve Broad - 5 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search