The 210g surface layer backed up with a 650g fabric will deliver a part with just under 1mm thickness and on something with narrow widths and angles like that it would feel quite sturdy.
Add in an additional layer of 300g fabric between those plies and it should feel very strong. If you want to be more certain, you can always add in small additional sections of the 300g fabric where you intend to attach anything. The 650g fabric will feel a little less compliant, so be certain to consolidate it well into the corners using a rounded tool of some description
|