Surface problems when coating with XCR skinning


Author
Message
Alvydas Jatkialo
A
Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)
Group: Forum Members
Posts: 10, Visits: 538
EDIT: I've used 150 and 220 foam backed sandpaper in step 5.

All work is done at 25C
I'm skinning some parts with XCR. Process is as follows:
1. Basecoat. 
2. I put carbon after basecoat reaches B-stage.
3. Everything goes into vacuum bag @ 20-30% vacuum overnight.
4. I put 3 coats of clear with 1h 30 min intervals as instructed in XCR datasheet
5. After 24 hours at room temp, and 8 hours at 60-70C in the oven I dry sand with 220 and 400 grit, wash off the dust, dry, degrease the surface.
6. Two more coats of clear resin similar as in (4)

Now the surface after two last coats has many craters. Is this called fish eyes?


How to prevent them? Last time I've tried acetone, silicone remover, and IPA alcohol on three different pieces before last two coats. All 3 pieces have exactly the same defects.
Edited 7 Years Ago by Alvydas Jatkialo
Warren (Staff)
Warren (Staff)
Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
It could be the surface needs more keying to give better adhesion.  

Also 25C may be a little too warm.  Although ideal for curing, the resin does thin out a lot above 20C which ironically would make fisheyeing worse so often working closer to 20C helps prevent this happening.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Hanaldo
Hanaldo
Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)Supreme Being (29K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Yeh it's really too finely finished. Finish with 180 grit at the finest before applying your final coats of resin.
Alvydas Jatkialo
A
Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)
Group: Forum Members
Posts: 10, Visits: 538
Thanks guys. Explanations seem logical.
Alvydas Jatkialo
A
Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)Supreme Being (127 reputation)
Group: Forum Members
Posts: 10, Visits: 538
Problems are gone when working at 20-21C.

I've made a mistake when writing first post. It appears I've been sanding with 150 and 220 foam backed sandpaper and not 220 and 400 as stated in the first post.
Warren (Staff)
Warren (Staff)
Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)Supreme Being (30K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Ok so it seems it was the reduced viscosity at higher temperatures. 

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search