Issue with hand layup carbon part


Author
Message
Damien
Damien
Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)Supreme Being (309 reputation)
Group: Forum Members
Posts: 32, Visits: 132
Hello,

I have an issue with my hand layout carbon fiber parts...

It looks like the resin does not fill in the carbon part really well...see photo

Here is my process:
- Mold with gel coat and easylease release agent (I have no problem releasing the part)
- Temperature 23-25 C
- This part (but I get the same with all parts) is 1 carbon  (1st layer) and 3 glass
- I use a 1.3:1 in weight for the amount of epoxy vs material
- I use the easycomposite roller to remove air bubbles etc...at each layer. This time, even, to try and see if it would help, I used a heat gun on each layer to get rid of micro-bubbles. But made no difference.
- Then I put a release tissue, a perforated film and a layer of special
foam to absorb the excess of epoxy.

- Vacuum bagging overnight

But still I get this...which gives me lots of work to give it a proper finish afterwards...

Any idea what I do wrong ?

Thanks !

Attachments
20190526_104715_resized.jpg (573 views, 867.00 KB)
Reply
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Nah the thing with infusion is that as long as you follow the process correctly and don't cut corners or rush, it will guarantee your part comes out perfectly (provided your mould is perfect of course). 

Hand layup is actually a more skilful technique, it is much more difficult to get things perfect because it is so much harder to eliminate voids.