Quick question regarding CS25 Silicone rubber


Author
Message
TURK
TURK
Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)Supreme Being (1K reputation)
Group: Forum Members
Posts: 101, Visits: 662
Hi guys,

I've finally managed to mould two ( Offside & Nearside ) headlight cover moulds using EC CS25 Silicone rubber.
The quality and definition of the finish is superb!  BigGrin

While I've been busy working on the next stage of the procedure ..................  casting 'Vac-Cast Epoxy Resin' into the silicone moulds,  a week has elapsed.

Now my silicone moulds have built-up an oily residue inside them!?  >>



My question is .............  can I simply 'wash out' with just a damp cloth the oily residue?
Or should I be cleaning the residue off with EC Mould Cleaner?

Other option I've read about are - Soapy water
Or even,  talcing powder!?

And,  how will this effect my Vac-Cast Epoxy Cast?

Any opinions ( comments ) greatly received.



Many thanks

TURK
T4 Concepts

Reply
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
It is definitely a mixing issue - have seen it with some of our condensation cure silicones when they are mixed off ratio, the oils from the unreacted components leach out. 

Be a bit careful, on the odd occasion the moulds with this problem will stick. Use your Mann Ease Release before casting into the mould.
Edited 6 Years Ago by Hanaldo
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
TURK - 6 Years Ago
TURK - 6 Years Ago
matthieutje65 - 6 Years Ago
TURK - 6 Years Ago
matthieutje65 - 6 Years Ago
TURK - 6 Years Ago
Warren (Staff) - 6 Years Ago
Hanaldo - 6 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search