Epoxy gelcoat vs polyster gelcoat


Author
Message
Hansson43
H
Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)
Group: Forum Members
Posts: 23, Visits: 2.1K
Hi, I wonder what’s the difference between epoxy gelcoat and polyester gelcoat ?
I have been working with epoxy gelcoat and epoxy resin for molds but find it rather expensive.
Is it possible to use polyster gelcoat with epoxy resin or do I have to use polyster resin with polyster gelcoat?

Best regards
Replies
Hansson43
H
Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)
Group: Forum Members
Posts: 23, Visits: 2.1K
Thanks good point I haven’t thought about that. I just bought what the guy I’m buying it from said would work.

Polyester does it shrink a lot ?
JasonFL
JasonFL
Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)
Group: Forum Members
Posts: 51, Visits: 707
Hansson43 - 1/9/2019 2:45:52 PM
Thanks good point I haven’t thought about that. I just bought what the guy I’m buying it from said would work.

Polyester does it shrink a lot ?


Yes polyester has potential to shrink a lot.  If you layup parts of your mould too thick they can get super hot (exothermic reaction) and cause voids as well as your gelcoat to pull away from the plug.  In general, epoxy moulds will retain the dimensions of your plug much better than polyester will.

A really cheap way to make epoxy moulds is to mix plaster, chopped glass, and epoxy to a clay like consistency.  Use this to build thickness after you have a few layers of cured woven cloth down. 


Jason
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Hansson43 - 6 Years Ago
matthieutje65 - 6 Years Ago
oekmont - 6 Years Ago
matthieutje65 - 6 Years Ago
Hansson43 - 6 Years Ago