Group: Administrators
Posts: 2.5K,
Visits: 8.5K
|
That part is way too dry of resin. Did you run the pump through the cure process? Without a proper resin break, you can suck out a lot of resin as it cures causing the very dry surface you see there. It can also happen if the resin shoots across quickly and you clamp off and in reality the resins shoot across the surface before its been able to soak in.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|