seense
seense
Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)
Group: Forum Members
Posts: 10, Visits: 138
I've had my first experiences with a PU resin (Xencast P6). I get decent castings but after demolding the casting is sweating an oily substance. Is this always the case with PU resins? I switched from epoxy to PU to increase production, but now I have to leave them sweating a few days and clean the parts.

I am casting a 15mm thick part in a 2-part mould CNC'ed out of Renshape 5173 pu toolingboard. The release agent is Easy Lease. I shake Part A thoroughly before mixing.
Reply
seense
seense
Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)Supreme Being (117 reputation)
Group: Forum Members
Posts: 10, Visits: 138
Thank you for the reply. I mix Part A + B very carefully (35+35 gr, accuracy: 0,1gr), pour it immediately and leave it. I found this on the smooth-on website:

https://www.smooth-on.com/support/faq/157/

Maybe it's just a bit too cold. For the next batch I'll try heating Part A + B to 23C before using it.