Paul (Staff) (19/07/2012)
Hi Leon,

You can run 2 layers of mesh to speed up the infusion, however this does have it's problems; if the resin flows too quickly through the mesh it will run ahead of the flow on the tool face this can lead to pinholes, the thicker the laminate is the worse this effect will become.

There is a trick to getting good results with a double mesh though; the resin flows very quickly at the start of the infusion (this is where the problem will be worst) to slow the infusion down you can restrict the flow of resin by not opening the line clamps fully at the beginning, as your resin flow begins to slow across the part you can open the clamps further to increase the rate. This will provide a quicker infusion overall.

Another thing you could try is to run more resin inlets onto the part this will allow a faster distribution without having to double up the mesh (which will consume quite a bit of resin) other than that there is trying to work somewhere cooler or mix the resin in a series of small batches as the resin infuses.

Thats some great work your doing... keep it up and keep us posted!


Thanks Paul,

considering the problem of pinholes I'll try to not open the line clamps fully at the begining. I interest about try to keep the resin in minimum temp to slower the reaction, is it ok to put the resin batch into ice batch during the infusion process?


Paul (Staff)
Paul (Staff)
Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)Technical Support (1.4K reputation)
Group: Administrators
Posts: 134, Visits: 614
Hi Leon,

You can run 2 layers of mesh to speed up the infusion, however this does have it's problems; if the resin flows too quickly through the mesh it will run ahead of the flow on the tool face this can lead to pinholes, the thicker the laminate is the worse this effect will become.

There is a trick to getting good results with a double mesh though; the resin flows very quickly at the start of the infusion (this is where the problem will be worst) to slow the infusion down you can restrict the flow of resin by not opening the line clamps fully at the beginning, as your resin flow begins to slow across the part you can open the clamps further to increase the rate. This will provide a quicker infusion overall.

Another thing you could try is to run more resin inlets onto the part this will allow a faster distribution without having to double up the mesh (which will consume quite a bit of resin) other than that there is trying to work somewhere cooler or mix the resin in a series of small batches as the resin infuses.

Thats some great work your doing... keep it up and keep us posted!

Paul Statham
Easy Composites / Carbon Mods - Technical
Leon
Leon
Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)
Group: Forum Members
Posts: 59, Visits: 606
Matt (Staff) (19/07/2012)
Amazing Leon! - You're another inspirational forum member (and customer) who's doing some really fine work and showing people what can be achieved with some effort and attention to detail. I like the 'WORKSHOP AREA - KEEP CLEAN' notes - I might put some of those up myself!

Both finished parts look top quality, I'm really pleased that after we did the video we're now seeing some fantastic parts being made. It's been a pleasure to supply you Smile


Thank's Matt,

I just do what you do on easycomposites watching your video hundred times, yes that was very very messy if I don't told my friend on the workshop to "KEEP CLEAN" very funny I think hahaha. 

I have a question Matt, My epoxy resin is quick to cure (20 minutes gell time), And I think is to slow when I reinforce large part, is it possible to using 2 layers of resin mess infusing to increase the process?

All the best

Leon 
Leon
Leon
Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)Supreme Being (443 reputation)
Group: Forum Members
Posts: 59, Visits: 606
Hi,

I'm from Indonesia, Surabaya-east java.

Thanks

Leon
Matt (Staff)
Matt (Staff)
Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)
Group: Forum Members
Posts: 680, Visits: 1.9K
Amazing Leon! - You're another inspirational forum member (and customer) who's doing some really fine work and showing people what can be achieved with some effort and attention to detail. I like the 'WORKSHOP AREA - KEEP CLEAN' notes - I might put some of those up myself!

Both finished parts look top quality, I'm really pleased that after we did the video we're now seeing some fantastic parts being made. It's been a pleasure to supply you Smile

Matt Statham
Easy Composites / Carbon Mods - Technical Sales
Warren
Warren
Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)Supreme Being (2K reputation)
Group: Administrators
Posts: 214, Visits: 782
the carbon kevlar looks good!!
SebRS
SebRS
Supreme Being (245 reputation)Supreme Being (245 reputation)Supreme Being (245 reputation)Supreme Being (245 reputation)Supreme Being (245 reputation)Supreme Being (245 reputation)Supreme Being (245 reputation)Supreme Being (245 reputation)Supreme Being (245 reputation)
Group: Forum Members
Posts: 29, Visits: 558
your work is really great Leon,

Pleasure to see this pics!
danishfx
danishfx
Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)Junior Member (7 reputation)
Group: Forum Members
Posts: 1, Visits: 31
Nice job leon..where u from?
Kevin-Lee
Kevin-Lee
Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)
Group: Forum Members
Posts: 44, Visits: 2.4K
You have done a fantastic job of those bonnets... Smile
Joe
Joe
Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)
Group: Forum Members
Posts: 310, Visits: 1.5K
Hi, Leon.

Awesome work ! Both looks great, but the Carbon/Kevlar looks killer Wink

Any chance to see pics of them when installed on the car?

 



 


    A $1000 electronic device will always protect a 10 cents fuse
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search