Hi I have sanded the pattern down up to 2000 grit. Then machine polished, but when polishing it making the surface worse with loads of small pin hole type bits. Iv tried slowing the polisher down. Any ideas? Or should I be hand polishing. I want it to look like glass when I Finnished Smile 

The gel coat is polyester tooling gel. 

I have uploaded a photo http://postimg.org/image/b5afyl3xt/


Thanks 
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
That looks like you've got porosity beneath your gelcoat surface and you're sanding into it, then the compound gets into the porosity and it becomes visible. 

Porosity can be a bit of an issue with polyester gelcoats. I would suggest trying a vinyl ester if you can get one. 