resistance to carburant


Author
Message
baleca
baleca
Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)
Group: Forum Members
Posts: 2, Visits: 5
hi, i need help
I'll make a motorcycle gas tank, and i need to know if there are any petrol resistant resin?
thanks
Edited 11 Years Ago by baleca
Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Hi,

Most epoxies have a good chemical resistance to petrol.  The problem is the ethanol within the petrol that slowly softens and degrades the resins.  This is especially the case with some bikes using composite tanks as the ethanol content has increased significantly in recent years meaning tanks that were fine are now causing problems on the bikes.

You need an ethanol resistant tank liner to use on your tank so it can be used with modern fuels. You need to look at specific tank lining phenolnovolac epoxies which are expensive and rare. The only one I’ve hear mentionedis GTS 1750 Tank Sealer which cropped up on the forum once.


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Edited 11 Years Ago by Warren (Staff)
carbonfibreworks
carbonfibreworks
Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
Warren (Staff) (02/06/2015)
Hi,

Most epoxies have a good chemical resistance to petrol.  The problem is the ethanol within the petrol that slowly softens and degrades the resins.  This is especially the case with some bikes using composite tanks as the ethanol content has increased significantly in recent years meaning tanks that were fine are now causing problems on the bikes.

You need an ethanol resistant tank liner to use on your tank so it can be used with modern fuels. You need to look at specific tank lining phenolnovolac epoxies which are expensive and rare. The only one I’ve hear mentionedis GTS 1750 Tank Sealer which cropped up on the forum once.


Yes the GTS1750 works well, the other option is to use ethanol free race fuel from company's like Sunoco etc.  Be careful not to make the tank too thin if you use a sealer, if the tank flexes the sealer may crack or break away from the carbon.
Chris
Carbon fibre works LTD

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
Edited 11 Years Ago by carbonfibreworks
baleca
baleca
Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)Forum Member (28 reputation)
Group: Forum Members
Posts: 2, Visits: 5
ok, i will try the GTS1750 resin, 
thanks for your time and help