Dear All

Can you clarify how to bond / laminate a sandwich panel from cured flat sheets of carbon fibre using Nomex honeycomb as the core please? Your Nomex honeycomb pages say to use epoxy resin. The aluminium honeycomb recommends a Permabond structural adhesive. Would I be better to use the structural adhesive for Nomex?

Would your recommendation change if I were to use one of your foam core materials.

Thanks in advance.

Regards,

John
Reply
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
The ET538 is specifically designed for bonding aluminium honeycomb so is correct for that application.

Normally in industry, higher volume work with nomex is likely to use film adhesives and an oven cure.  This is not always practical for small scale or DIY projects.

A batch of epoxy resin can be mixed and spread onto a surface so that the honeycomb can be dipped into it, coating the contact areas with resin without resulting in un-needed resin in none-contact areas. The honeycomb can then be placed onto the composite sheet and the first side allowed to cure. Once cured, repeat the process by dipping the other side of the honeycomb into resin and weighting it down onto the other skin.

A foam core is a bit easier as you can simply spread the resin onto the foam core using a brush thus minimising resin wastage.


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search