Hello all,

I hope someone could help me with my "little" problem(sorry for the errors, english is not my mother language).

I just finished my mould that I made following the videos on the easy composit home page using the uni mould kit products. And I don't think I missed a step or did something wrong, but on one spot I got something strange. Something went wrong and I don't know what or why. It's like there's been some chimical reaction that gave this white layer so that the gel coat couldn't attach as it should.

I join some pictures to show you.
What should I do? Can I polish this spot then apply a thin layer of gel coat and repolish or is this a bad idea? I just hope I don't have to start all over.

Thanks in advance
Attachments
IMG_1872.JPG (618 views, 1.00 MB)
IMG_1870.JPG (583 views, 1.00 MB)
IMG_1871.JPG (464 views, 1.00 MB)
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
From the pictures it looks like something on the surface of your plug may have reacted with the gelcoat. What is your plug made from and what release agent did you use? Is the plug surface now damaged? Was it difficult to demould?

When the exotherm kicks in the temperatures get well over 60 degrees C more than enough to soften paints and even some plastics causing major problems.

Warren

Carbon Copies Ltd
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
Looks like a problem called Alligatoring,
Look for it on google Smile

Might be a problem with mixing ratios, a to thin coat of gelcoat or problems with the releaseagent (at least that was the cause of the problem when I had it once) 

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Might be alligatoring but its uneven nature leads me to think some kind of contamination or solvant reacted with the gelcoat.

You can fix it in the same way any gel coat repair is done.  Sand it out and refill with fresh gelcoat mixed with a little Solution MW Wax Gelcoat Additive to prevent the cured resin being tacky. Then once cured, sand flat with surrounding gel and polish back up.


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Adelbolide
Adelbolide
Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)
Group: Forum Members
Posts: 16, Visits: 112
Hello all,

thanks a lot for your help and explications

To answer your questions, I followed the tutorial, but there was a crack on the surface, so I filled it with the yellow filling wax and gel coated it over. And I think you're right, with the exotherm kicking in the wax melted and reacted with the release agent and gel coat.

I'm glad I can repair it. Thank s a lot for your advice
Adelbolide
Adelbolide
Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)
Group: Forum Members
Posts: 16, Visits: 112
Warren (Staff) (13/10/2014)You can fix it in the same way any gel coat repair is done.  Sand it out and refill with fresh gelcoat mixed with a little Solution MW Wax Gelcoat Additive to prevent the cured resin being tacky. Then once cured, sand flat with surrounding gel and polish back up.


Hello,

I bought the Solution MW Wax Gelcoat Additive but I'm not sure if I should use the catalyst with the gelcoat and the additive or not.

Thanks in advance
wozza
wozza
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
You still need the catalyst, the wax additive rises to the surface creating an air seal so that the gelcoat fully hardens.

Warren

Carbon Copies Ltd
Edited 11 Years Ago by wozza
Adelbolide
Adelbolide
Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)Supreme Being (149 reputation)
Group: Forum Members
Posts: 16, Visits: 112
thanks for your help
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search