Catalyst doesn't matter. You can mix it by weight or volume, the difference is negligible. I prefer to mix by weight, simply because I don't then have to be careful pouring quantities to a specific line. 
ajb100
ajb100
Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)
Group: Forum Members
Posts: 346, Visits: 4.4K
Mixing is done by weight, not volume, so 100g with 2g MEKP.
remodovakhin
remodovakhin
Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)
Group: Forum Members
Posts: 2, Visits: 14
Thanks for the reply Bro!! So i had another doubt..when they say add 2% catalyst to the resin, does that mean i should add 2ml of catalyst to a 100ml batch of resin?? Your reply is highly appreciated bro! btw i am attaching a pic of our car to be made here..it is to be a one piece mould.
Attachments
1.JPG (386 views, 31.00 KB)
3.JPG (370 views, 14.00 KB)
Dravis
Dravis
Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
Hi ..

Watch as many of the EC tutorials as you have time for... they will tell you a lot.. BigGrin

Take a look at the "car bonnet" vids ... part 1 and 2 deal with "plug" and Mould" making.

Also search Youtube for vids showing mould building and wet-lay of boats, cars and even planes.. Rolleyes

When working with Polyester and Vinylester resins, work in a well ventilated area and use a mask... Styrene vapours are very nasty stuff...

And .. No, the Polyester and Vinylester resins you have only require the MEKP/MEPOXE catalyst around 1,5% to 2 % (normally)

(check the datasheets/info for the resins.)

Good luck!

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
remodovakhin
remodovakhin
Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)
Group: Forum Members
Posts: 2, Visits: 14
Hi guys! I am a noob and newbie in Fibreglass stuff. I am a fourth year engineering student actually. We are making the body of our car for the Shell Eco Marathon actually. This is also our first time. the plan is to first build a plug and then make a female mould using fibreglass and then applying carbin fibre on the insides on this mould to get the final carbon fibre car body. SO we have bought a few fibreglassing items:-

I have purchased pre-accelerated Vinylester Resin Crystic VE679 PA, pre-accelerated Polyester Resin Crystic RTR 4000PA, Crystic GelCoat 12 PA Pine Green, Surface Primer Grey Nord 210 lAQUE, Surface primer Nord 230, methylene Chloride (like acetone) and 450g/m2 CSM glass matt. I also have the catalyst MEPOXE. Now my problem is i am a little confused about these chemicals. I want to build a fibreglass female mould using these chemicals. So firstly we are planning to build a plug using mdf and pour foam. Then the plan is to apply putty or body filler to fill in pores and gaps on the plug surface, this will then be sanded. Then i would apply 'Mould kanstik sealer' to seal porosities. Then next i would apply the gelcoat, followed by ... I am lost then. Can someone here please guide me on how i can use the above chemicals to build my plug to good smoothness and then create my female fibreglass mould. i cannot thank you enough for your help! 

Also some of my questions are-  Do the Vinylester and the Polyester resins mentioned above require a hardener chemical as well to cure or is it just enough to add the catalyst? And how much catalyst am i to add normally? Also what is the difference between the Vinylester resin and the polyester resin? Are these chemicals used together or do i just use one of them to put on the fibreglass? 

Your answers are highly appreciated!

Thanks and Regards
Hoping to hear from you PROS soon!
BoostSamurai
BoostSamurai
Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)
Group: Forum Members
Posts: 34, Visits: 413
Thanks guys Smile  I'll get some more supplies (microballoons etc) and give it another shot soon.

It's fantastic when people post up their successes but I think it's also useful for noobs like me to post up the failures as well, that way others can hopefully learn from our mistakes, rape or no rape Tongue

JZX World Forums
Edited 11 Years Ago by BoostSamurai
kidpaint
kidpaint
Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)Supreme Being (778 reputation)
Group: Forum Members
Posts: 99, Visits: 676
Keep it up! Looks like you're headed in the right direction.

Violent rape....what 😳
ajb100
ajb100
Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)Supreme Being (2.6K reputation)
Group: Forum Members
Posts: 346, Visits: 4.4K
George Sychrovsky (29/06/2014)
Looks like a violent rape to me


Erm, ok?
George Sychrovsky
George Sychrovsky
Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)
Group: Forum Members
Posts: 24, Visits: 1.6K
Looks like a violent rape to me


---------------------------------------------------------------------
Disclaimer opinions of others will vary depending on what they are selling
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Airbrush should work, it will just take awhile to apply. 